◆ Rebuild

Part 2 · Earth and Fire

Tar, Pitch and Glue

How to cook birch bark and resinous pine into sticky black tar, boil it down to pitch, and mix pitch with charcoal and dung into a glue that holds a stone point on a shaft. Tar and pitch also waterproof boats, roofs, rope and pots.

Difficulty
●●●●●
Time
Half a day for a pot of birch tar; two to four days for a pine tar pit; an hour to make pitch glue
Steps from zero
4 prerequisites →

You need first

CharcoalPottery

This unlocks

Glues and Adhesives
The full path from nothing — 4 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Charcoal
  4. Pottery
  5. Tar, Pitch and Glue

Do them roughly in this order. See it on the tech tree →

Why it matters

Tar is the oldest man-made material that is not just a shaped stone or stick. It is a glue that sets as it cools, a waterproofing that does not wash off, and a preservative that stops wood and rope from rotting. With it you can:

Making tar uses the same trick as Charcoal — heating wood without air — and the same clay pots as Pottery. If you can make those, you can make tar.

How it works

Tar is the thick, dark liquid that comes out of wood or bark when it is heated without enough air to burn. Between about 250 °C and 400 °C, the wood breaks apart. The gases and vapours that escape include water, sour "wood vinegar" (mostly acetic acid), burnable gas, and oily tars. If those vapours can run away from the heat and cool, they condense into liquid. What is left behind is charcoal. This is called dry distillation.

Two natural materials give far more tar than ordinary wood:

  • Birch bark — the white, papery outer bark. It is full of a waxy substance (betulin) that turns into a thick, black, very sticky tar.
  • Resinous pine — old pine stumps, roots and the bases of dead branches, soaked with resin over many years. This is fatwood (see Fire): amber-coloured, heavy, sticky, smelling of turpentine. It gives brown-black pine tar.

Then there are two related materials:

  • Pitch is tar that has been boiled down. Boiling drives off the thin oils, leaving a material that is soft and sticky when warm and stiff or even glass-hard when cold. The longer you boil, the harder it gets.
  • Rosin is pine resin (the sap that oozes from cuts in a living pine) that has been melted and strained, driving off its turpentine. It is clear, amber and brittle.

Glue from pitch works because it is thermoplastic: heat it and it flows into every crack; let it cool and it grips. Pure pitch or rosin is brittle — a knock shatters it. Mixing in a filler (fine charcoal powder) and fibre (dried dung) stops cracks from spreading, the way straw strengthens mud brick. A little beeswax or fat makes it tougher and less brittle in cold weather.

What you need

Item Amount Notes
Birch bark, outer white layer 0.5–1 kg (a big armful) Dry; from dead or fallen trees
or Fatwood split into sticks 5–20 kg for a pot; 0.5–2 m³ for a tar pit The more resin, the more tar
Two clay pots One 2–4 litre pot, one smaller pot whose mouth fits under it Fired, sound, unglazed is fine (see Pottery)
Clay A bucketful To seal joints and lids (see Finding and Preparing Clay)
Firewood An armful or two Dry, wrist-thick
Pine resin A double handful for glue Collected from wounds in pine trees
Charcoal A handful, ground to powder See Charcoal
Dried herbivore dung A handful Rabbit, deer, sheep, cow or horse, dried and crumbled
Beeswax or tallow A walnut-sized lump (optional) See Beekeeping and Lamps and Candles
A small pot or shell, sticks, flat stones For melting and mixing glue

Where to find it

  • Birch grows in cool northern forests, in mountains, on heaths and on the edges of bogs. Its bark is white to cream, peeling in thin horizontal sheets marked with dark slits. Fallen birch trunks often rot inside while the bark stays whole as a tube; pull it off in sheets. Peel only loose bark from living trees — taking a full ring kills the tree.
  • Fatwood is found in old pine stumps, especially where a pine was cut or blown down years ago; in the knots and roots; and at the base of dead branches on living pines. Split a stump: fatwood is darker, translucent at the edges, heavy, and sticky, and smells strongly of turpentine. Light a splinter — fatwood burns with a smoky, sooty, candle-like flame. Scandinavian tar-makers "prepared" pines by stripping bark from the lower trunk of living trees, leaving a narrow living strip; over five to seven years the trunk filled with resin. If you will stay in one place for years, you can do the same.
  • Pine resin oozes from wounds in pine, spruce, fir and larch. Collect old hardened lumps, or cut a shallow V into the bark (never all the way round) and fix a cup or a bark funnel below. A tree gives a cupful in a few weeks in summer.
  • Dung: dry pellets from rabbits, deer or sheep are ideal — they are mostly fine chewed plant fibre.

Method 1: Birch-bark tar in a double pot

Lidsealed with clay Rolled birch barkpacked tight, upright 3–5 holesabout 5 mm each Clay sealno air may get in Tar collectspot kept cool in earth Fireall round, 1½–2 hours Ground levelrim of lower pot
Fig. 1 The double-pot method in cross-section. Rolled birch bark is sealed in the upper pot, which has small holes in its base. The fire heats it from above and the sides; tar runs down through the holes into the cool lower pot buried in the earth.

This is the simplest way to make good tar in useful amounts.

  1. Make holes. Using a hot pointed stick or a sharp stone, drill 3–5 holes about 5 mm across in the bottom of the upper pot. (Better still, make them before firing the pot.)
  2. Fill it. Roll strips of birch bark tightly into little scrolls, the size of a thumb, and pack them standing upright into the upper pot until it is crammed full. The tighter the packing, the more tar.
  3. Bury the collecting pot. Dig a hole and set the smaller pot in it so its rim is level with the ground. Pack earth firmly around it. The earth keeps it cool, so tar condenses in it instead of burning.
  4. Join them. Set the upper pot on top so its holes are over the mouth of the lower one. Seal the joint all round with a thick ring of wet clay, and heap earth against it. Close the upper pot with a lid (a flat stone or sherd) and seal that with clay too. No air must get in — air lets the bark burn instead of distilling.
  5. Fire. Build a fire all round and over the upper pot, but keep the ground and the lower pot cool. Keep it burning strongly for 1½–2 hours. Steam and then thin yellowish smoke may leak from the clay joints; patch the leaks with more clay. When smoke stops coming from the joints, the bark is spent.
  6. Cool. Let the fire die and leave everything to cool for at least an hour. Opening it hot lets air in, and the charred bark may flare up.
  7. Collect. Break the clay seal and lift off the upper pot. The lower pot holds dark brown to black liquid tar, often with a watery layer on top. Pour off the water. Inside the upper pot are curls of bark turned into charcoal.

Yield. Expect roughly 5–15% of the weight of the bark as tar: a well-packed 3-litre pot (about half a kilogram of bark) gives perhaps a small cup, 30–60 ml. That is plenty to haft a dozen arrowheads.

Tip Without pots. People made birch tar long before pottery. Roll a strip of birch bark and set it burning slowly beside a smooth, cool stone, so the smoke and flame lick across the stone. Black tar condenses on the stone; scrape it off with a flint flake and repeat. It is slow — a few grams an hour — but needs nothing at all.

Method 2: Pine tar in a tar pit

Lit at the topa few small vent holes Turf, then 10–15 cm earthgrass side down Split fatwoodstacked tight, sloping inward Charring creeps downover one to three days Clay-lined funnel1.5–2 m across, 50–70 cm deep Outlet pipesloping down the hill Tar potchange when full
Fig. 2 A small tar pit on a slope. Split fatwood is stacked in a funnel-shaped pit lined with clay, covered with turf and earth, and lit at the top. It chars downward; tar runs down the funnel and out through a pipe into a pot below.

For larger amounts — enough to tar a boat or a roof — build a tar pit, as Finnish and Swedish farmers did for centuries. It is a Charcoal mound built over a funnel.

  1. Choose a slope of firm, clayey ground. Dig a round funnel-shaped pit 1.5–2 m across and 50–70 cm deep at the centre, with smooth sides sloping in at about 30°.
  2. Line the funnel with 5 cm of well-wedged clay, or with overlapping sheets of birch bark under a skin of clay, smoothed so tar can run. It must not soak into the soil.
  3. Lay the outlet. From the bottom centre, lay a pipe running downhill and out through the slope: a hollowed log, a line of clay pipes, or a channel lined with clay and covered with flat stones. At its outer end, dig a pit for the collecting pot or barrel. Cover the inner mouth of the pipe with a small grid of sticks so wood does not block it.
  4. Split the fatwood into sticks 30–60 cm long and wrist-thick. Dry them for a few weeks.
  5. Stack. Lay the sticks tightly, radiating from the centre like the spokes of a wheel and sloping down toward the middle, building up into a dome about 1 m high. Pack small pieces into the gaps — tight packing gives more tar.
  6. Cover. Lay turf over the whole dome, grass side down, then 10–15 cm of earth, just as for a charcoal mound. Leave the top 20–30 cm open.
  7. Light the top and let it catch well, then partly cover it, leaving a few finger-sized vent holes around the top. The fire must creep slowly downward, charring the wood and driving the tar down ahead of it.
  8. Tend it day and night. Watch the smoke: thick white smoke is good. If you see flame breaking through, the wood is burning — close that hole with earth. If smoke stops and the mound goes cold, open a new vent a little lower. Move the vents down the sides as the burn works down.
  9. Collect. After several hours the first liquid runs: a thin, sour, brownish water ("tar water" or wood vinegar). Then comes thin brown tar, and later thick, dark tar. A small pit runs for one to three days. Change the collecting pot when it fills.
  10. Finish. When tar stops running, seal all vents with earth and let the mound cool for a day. Dig out the charcoal — a valuable by-product.

Very resinous stump wood can give 10–20% of its weight as tar; ordinary pine gives much less. You can also make small amounts of pine tar in the double pot of Method 1, packed with fatwood splinters, or by leading the smoke pipe of a charcoal retort into a cool pot (see Charcoal).

Making pitch and rosin

Pitch from tar.

  1. Put the tar in a pot no more than one third full. Work outdoors, with a flat lid or sherd ready beside you.
  2. Heat it gently over small embers, stirring with a stick. Water spits and bubbles off first, then the tar thickens and smokes heavily.
  3. Test it every few minutes: drip a little into cold water and squeeze it.
    • Sticky and pliable, like soft chewing gum → soft pitch, for caulking and pot linings.
    • Firm, takes a fingernail dent slowly → medium pitch, for glue.
    • Snaps like glass → hard pitch. If it is too hard, stir in a little fresh tar or fat.
  4. Expect the tar to lose a third to a half of its volume.

Rosin from pine resin. Melt raw resin gently with a little water in a pot. Strain it while hot through a coarse cloth or a pad of dry grass to remove bark, needles and insects. Keep heating gently until the bubbling stops and it smells less of turpentine. Poured onto a wet stone, it sets into clear amber lumps. (The turpentine that boils off can be caught by Distillation — it is a valuable solvent; see Ether, Acetone and Solvents.)

Making pitch glue

A good all-purpose hafting glue, by volume:

Ingredient Parts Job
Pine resin or rosin (or birch tar boiled down a little) 4–5 The glue
Charcoal, ground to fine powder 1 Filler; stops cracking, makes it black and less sticky to hands
Dried dung, rubbed to fine fibre 1 Fibre; reinforces like straw in mud
Beeswax or tallow ½ (optional) Makes it less brittle, especially in cold
  1. Melt the resin slowly in a small pot or a shell set on the edge of the embers. Do not let it boil or catch fire. If it flames, cover it at once with a sherd.
  2. Stir in the charcoal powder a little at a time, then the dung, then the wax.
  3. Test: dip a stick, let the blob cool for a minute, then press it with a thumbnail. It should dent, not shatter; and it should not stay soft and sticky. Too brittle → more wax or fat. Too soft → more resin and charcoal, and cook a little longer.
  4. Wind the warm mixture onto the end of a stick into a ball — a pitch stick. It keeps for years. To use it, warm the end over a fire until it drips, and dab it where you need it.

Hafting a point. Split or notch the shaft, warm both the stone and the shaft, and fill the slot with melted glue. Press in the point. While the glue is warm, mould it smooth with wet fingers (it will not stick to wet skin). Then wrap the joint with wet sinew or fine Cordage and Rope and coat the wrapping with a thin layer more. The sinew shrinks as it dries and the glue locks it.

1. The point sits in a slot filled with warm glue (cut-away) 2. The joint wrapped with wet sinew, then coated with glue Glue fills the slotwarm stone and shaft first Stone point Shaft tang hidden inside Pitch stickwarm the tip to use Sinew wrapping, 3–4 cm longshrinks as it dries and locks the joint Thin coat of gluesmoothed with wet fingers
Fig. 3 Hafting with pitch glue. Glue fills the slot; a wrapping of sinew locks the point in place; a thin coat of glue seals the wrapping.

Hide glue is the other great early glue. Simmer scraps of rawhide, skin trimmings or fish skins gently in water for several hours (do not boil hard), strain, and boil the liquid down until it sets into a jelly when cold. Used warm, it glues wood very strongly — but it softens in water. Pitch is waterproof; hide glue is not. See Glues and Adhesives.

Using tar and pitch

  • Caulking a boat. Hammer twisted fibre (old rope picked apart, moss, or animal hair) soaked in tar into each seam with a blunt chisel, then pour or brush hot soft pitch over it.
  • Wood preservation. Paint pine tar on boat hulls, shingles, posts and wooden roofs. Warm it so it soaks in. Scandinavian builders thinned it with an equal amount of linseed oil (see Oils and Pressing). Repeat every few years.
  • Rope. Pull rope slowly through a pot of warm, thin tar and hang it to drip. Tarred rope resists rot and water for years.
  • Pots. Warm the pot by the fire and swirl hot soft pitch around the inside. It seals the pores for storing liquids — but not for cooking (see Pottery).
  • Axle grease. Mix tar and animal fat half and half (see Lubricants and Greases).

How to tell it worked

  • Birch tar is black, glossy and extremely sticky, and smells of smoky leather. Pine tar is dark brown to black, thinner, and smells of smoke and turpentine.
  • Pitch hardens as it cools. A drop in cold water can be picked up as a solid bead.
  • Glue sets within a minute. A properly hafted point cannot be twisted out by hand, and survives an arrow hitting a log.
  • Waterproofing: a pitched pot holds water without sweating; a tarred board beads water.

Note Troubleshooting. No tar in the lower pot → the upper pot never got hot enough (build the fire higher and longer), or air got in and the bark burned (better clay seals). Check that the holes are not blocked. Tar full of ash and grit → holes too big, or bark crumbled. Strain the tar through cloth while warm. Thin, watery, sour liquid → that is the first run; separate the water and boil the rest down to thicken it. Pitch too brittle; glue cracks off in the cold → overcooked; add a little fresh tar, wax or fat. Glue stays soft and sticky → undercooked, or too much wax; cook longer, add resin and charcoal. Glue does not grip the stone → the stone or shaft was cold, wet or greasy. Warm both before gluing. Tar pit burns to ash with little tar → too much air; fewer and smaller vent holes, thicker earth cover.

Dangers

Danger Tar and pitch burn — and stick. Hot pitch clings to skin and keeps burning. Cool a pitch burn at once under cold water for 20 minutes; do not pull the pitch off. Once cold, soften it away later with fat or oil. Tar, pitch, resin and turpentine vapour all catch fire easily: boil them only outdoors, in a pot no more than one third full, with a lid ready to smother flames. Never pour water on burning tar — it spatters burning tar everywhere. Smother it with a lid, earth or sand.

  • Boil-over. Water hidden in tar makes it foam up suddenly when heated. Heat slowly and stir.
  • Smoke and fumes. Tar smoke contains substances that cause cancer after long exposure, and it irritates eyes and lungs. Work upwind and outdoors, and do not make tar a daily indoor job. Wash tar off skin with fat, then soap.
  • Carbon monoxide. A tar pit, like a charcoal mound, makes deadly invisible gas. Never sleep in a hollow beside one or downwind of it.
  • Forest fire. Tar pits burn for days. Clear all dry vegetation for 5 m around and keep water and earth ready.
  • Dung. Handle it with care and wash your hands; it can carry disease. Use only dry, old pellets, and never in anything near food.

What this unlocks

Tar and pitch make Rafts and Canoes and Boats and Sails watertight, preserve Roofs and rope, grease axles, and seal barrels. Rosin becomes solder flux (Soldering and Brazing), varnish (Pigments, Paints and Varnish) and the grip on a fiddle bow (Violins, Guitars and Harps). Pitch makes the laps that polish Lenses and Mirrors. Pitch glue, hide glue and their relatives lead to the full range of Glues and Adhesives. Much later, tar from Coal and Coke (Coal Tar Chemicals) and Petroleum and Refining becomes the starting point of dyes, medicines and Early Plastics.

How it was first done

Tar is older than our species. Neanderthals made birch-bark tar to glue stone tools to handles: tar-coated flakes from Campitello in Italy are about 200,000 years old, and lumps of birch tar with the imprint of a tool and a fingerprint were found at Königsaue in Germany, more than 40,000 years old. They made it without pots — probably by condensing it on stone, as in the tip above. Lumps of chewed birch tar with children's tooth marks survive from Stone Age Scandinavia, about 10,000 years ago. The Iceman found in the Alps (about 3300 BC) carried arrows with points glued in with birch tar. Greeks and Romans made pine pitch on a large scale for ships and wine jars. From the Middle Ages until the 1800s, Sweden and Finland burned pine tar in pits like the one in this chapter and sold it by the barrel to the navies of Europe; in the 1800s Finland was the largest tar exporter in the world.

Source: content/entries/earth/tar-and-pitch.md