◆ Rebuild

Part 2 · Earth and Fire

Mortar and Concrete

How to turn lime, sand, gravel and a little volcanic ash or crushed brick into mortar that binds walls, waterproof linings for cisterns, and Roman concrete that sets under water and lasts two thousand years — with ratios, mixing, curing and simple strength tests.

Difficulty
●●●●●
Time
An hour to mix a batch; a week of curing before loading; months to reach full strength
Steps from zero
4 prerequisites →

You need first

Lime

This unlocks

Arches, Vaults and DomesStone MasonryLaying Tiles and MosaicsRoads and Bridges

Objects made here

concretemortarcistern
The full path from nothing — 4 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. The Kiln
  4. Lime
  5. Mortar and Concrete

Do them roughly in this order. See it on the tech tree →

Why it matters

A wall of stacked stones stands only as long as gravity and friction keep it there. Bind the stones or bricks with mortar and the wall becomes one solid piece: it can be taller and thinner, it keeps out wind and water, and it can carry arches, floors and roofs. Mix mortar with broken stone and pour it into a mould and you have concrete — artificial rock in any shape you want: foundations, floors, cisterns, harbour walls, domes.

The Lime chapter shows you how to burn and slake lime and make the simplest mortar. This chapter goes further:

  • How to choose and grade sand so your mortar is strong.
  • How to make hydraulic mortars that set without air — inside thick walls, in wet ground, even under the sea.
  • How to make Roman concrete from lime and volcanic ash or crushed brick.
  • How to mix, place, cure and test it.

It leads to Stone Masonry, Foundations and Floors, Arches, Vaults and Domes, Wells and Cisterns, Roads and Bridges, Portland Cement and finally Reinforced Concrete.

How it works

Binder and aggregate

Every mortar and concrete has two parts:

  • The binder — the glue: lime, gypsum (Gypsum and Plaster of Paris) or cement (Portland Cement). It starts as a paste and hardens.
  • The aggregate — the filler: sand in mortar, sand and gravel or broken stone in concrete. Aggregate is cheap, does not shrink, and carries most of the load. The binder's job is to coat every grain and fill the gaps between them, and no more. Too much binder shrinks and cracks; too little leaves holes.
+ 1. Fill with dry sandShake it down. The grains touch,but there are gaps between them. 2. Pour in measured wateruntil it just reaches the top. Thewater used is the empty space —about one-third with good sand. 3. Binder fills the gaps1 part lime : 3 parts sand. The mixis hardly bigger than the sand,as the lime goes into the gaps. 3 sand1 lime about 3 of mortar
Fig. 1 The voids in sand. Even tightly packed sand is about one-third empty space. The ideal mortar has just enough binder to fill those gaps and coat every grain — which is why the classic ratio is one part binder to three of sand.

Three ways to set

  1. Air-setting (non-hydraulic) lime — ordinary slaked lime hardens only by taking carbon dioxide from the air, turning slowly back into limestone (see Lime). It is soft, flexible, and slow: weeks to firm up, years to finish. It never sets under water or deep inside a massive wall.
  2. Hydraulic lime — lime burned from limestone that contains clay. During burning, the clay's silica and alumina combine with some of the lime into compounds that react with water — not air — to form hard crystals, much like cement. It sets in damp places and under water.
  3. Lime plus pozzolan — a pozzolan is a material rich in reactive silica and alumina that does nothing on its own, but reacts with slaked lime and water to make the same hard, water-resistant compounds. Named after Pozzuoli near Naples, where the Romans dug the best volcanic ash. Volcanic ash, some volcanic tuffs (trass), pumice, and clay that has been fired — crushed brick and pottery — are all pozzolans.

Methods 2 and 3 are what made Roman concrete possible. Ordinary lime mortar is what held together nearly every brick and stone building in the world for thousands of years.

What you need

Item Amount (for about 1 m³ of mortar) Notes
Lime putty 0.3 m³ (about 300 litres) Matured at least two weeks; see Lime
Sharp sand 0.9 m³ Washed, well graded (below)
Pozzolan 0.3–0.6 m³ for hydraulic mixes Volcanic ash, trass, or crushed fired brick or tile, sieved
Gravel or broken stone For concrete: about twice the sand volume 1–6 cm pieces, clean
Water As little as possible Clean; never seawater for lime mortar in walls you will live in (salt draws damp) unless making marine concrete
Mixing board 2 × 2 m Planks, flat stones or a hard clay floor
Hoes, shovels, rammers A rammer is a heavy wooden block (5–10 kg) on a handle
Gauge boxes or baskets Any container used to measure parts by volume
Formwork Planks and stakes, or a stone or brick facing that stays in place
Sacking, straw, mats To keep fresh work damp and shaded

Where to find it

  • Sand. Riverbeds and banks, old river terraces, pits in glacial gravel, crushed sandstone. Sharp (angular) grains lock together better than round ones: rub some between your palms — sharp sand feels gritty and "bites", round beach or dune sand feels smooth and rolls. Beach sand must be washed several times in fresh water to remove salt.
  • Gravel. Riverbeds, the insides of river bends, glacial deposits, broken stone from Quarrying and Cutting Stone.
  • Volcanic ash and tuff. In volcanic regions: soft, pale grey, yellow, pink or brown beds that crumble to a gritty powder and do not fizz with acid (see Rocks and Minerals). The best ones are very fine and feel slightly harsh, not slippery like clay.
  • Crushed brick and pottery. Broken Bricks, roof tiles and pots, especially those fired at a dull to bright red heat (600–900 °C). Very hard, glassy, high-fired brick is a weaker pozzolan. You can also fire lumps of clay deliberately for the purpose (see "Make your own pozzolan" below).
  • Clayey limestone for hydraulic lime: darker grey or bluish limestone that fizzes but leaves a muddy residue when a fragment is dissolved in strong vinegar. Thin limestone beds between shales are often clayey. See Portland Cement.

Testing sand

  1. Cleanliness — the jar test. Fill a clear jar or glass vessel one-third with sand, add water to two-thirds, shake hard, and let it stand an hour. Clay and silt settle in a layer on top of the sand. If the layer is more than about one-twentieth of the sand's depth, wash the sand: stir it in a tub of water, pour off the muddy water, repeat until the water runs clear.
  2. Salt. Taste it. Salty sand must be washed.
  3. Grading. Good sand has a mix of sizes from fine to coarse (up to about 3–5 mm), so small grains fill the gaps between big ones. Sieve out stones over 5 mm for mortar.
  4. Voids — the bucket test. Fill a bucket to the brim with dry sand, shaking it down. Then pour water slowly into it from a measured vessel until water just reaches the surface. The volume of water is the volume of empty space between the grains. With good sand it is about one-third of the bucket. That is how much binder you need: one part binder to three of sand. If your sand has more voids (say 40%), use a little more binder (1 : 2½); if fewer, a little less.

Method 1: Better lime mortar

The basic mix is given in Lime: 1 lime putty : 3 sand by volume. Two improvements:

Hot-mixed mortar. Much Roman and medieval mortar was made by slaking quicklime directly in damp sand, which gives a stickier, quicker-setting mortar with small white lumps of lime in it. Spread 3 parts damp sand in a ring, put 1 part crushed quicklime (pea- to walnut-sized) in the middle, sprinkle with water, and cover it with the sand. It will steam and get very hot. After an hour or two, turn it over and mix well, adding a little water. Use it within a day or two, or let it mature covered for a week. Wear eye protection — see Dangers and Lime.

Fibres and additives. For renders (outside coatings) and plasters, mix in clean animal hair or chopped straw, about a double handful per bucket, to stop cracking. Chinese builders added cooked sticky rice soup to lime mortar for city walls and tombs from about 1,500 years ago; a thin rice or starch soup in the mixing water makes a tougher, more water-resistant mortar.

Method 2: Hydraulic lime

If you have clayey limestone, burn it exactly as ordinary lime (Lime), but only to bright cherry–orange heat (900–1,000 °C) and pick out any glassy, fused lumps. Then:

  1. Slake to powder, not putty. Sprinkle it with about a third of its weight in water and cover with sand (see Lime). Hydraulic lime slakes slowly and quietly — sometimes taking hours or days — with little heat. That slowness is a sign of hydraulic power. Never store it as putty: under water it would set.
  2. Sieve out unslaked lumps through a fine basket. Grind them and add them back, or discard them.
  3. Mix 1 hydraulic lime : 2½–3 sand, with just enough water to make a workable paste. Use it within a few hours — it starts to set.
  4. The test. Make a ball of the paste the size of an egg, let it stiffen for a day, then put it in a bowl of water. A strongly hydraulic lime holds together and is hard to scratch with a fingernail after a week; a weak one softens or crumbles.
Clay in the limestone Lime made Sets under water in
Under 5% Ordinary (air) lime Never
5–12% Feebly hydraulic 2–3 weeks
12–18% Moderately hydraulic About a week
18–25% Eminently hydraulic A few days
25–35% Natural cement — see Portland Cement Hours

Method 3: Lime and pozzolan

This needs no special limestone, only ordinary lime plus a pozzolan.

  1. Prepare the pozzolan. Dry it, crush it, and sieve it. For mortar, everything should pass a fine sieve or cloth of about 1 mm; the finer the powder, the more it reacts. Keep coarser bits (up to 5 mm) as part of the sand.
  2. Mix. Good starting ratios by volume:
    • For ordinary hydraulic mortar: 1 lime putty : 1 pozzolan : 2 sand.
    • For work in water or the sea (following the Roman writer Vitruvius): 1 lime putty : 2 volcanic ash, no sand.
    • For waterproof cistern and bath linings (Roman opus signinum or cocciopesto): 1 lime putty : 2 crushed brick or tile, mixed from fine powder to pieces of about 5 mm.
  3. Beat it thoroughly on the board with hoes or by treading, for 15–20 minutes, adding water sparingly. It should be stiff and sticky.
  4. Use it within a few hours, and keep it damp afterwards (below).

Tip Make your own pozzolan. Burn ordinary clay — dried, broken lumps — in a The Kiln or open fire to a dull red heat (about 700–800 °C) for two or three hours, then crush and sieve it. Pale, low-iron clays (kaolin, see Finding and Preparing Clay) give the most reactive powder. Test every batch with the underwater ball test before you trust it in a cistern or foundation.

Method 4: Concrete

Concrete is mortar with coarse stone in it. Roman builders did not pour it like modern concrete; they laid it in layers and rammed it.

Rammer5–10 kg wooden block Mortar layer5–10 cm, spread first Stone layer3–15 cm pieces, wetted,rammed into the mortar Facingstone or brick laidin mortar; stays 30–60 cmper day Or: plank formworkties across the top Stakes brace the plankswet them first; strike after 1–2 weeks
Fig. 2 Building a Roman-style concrete wall. Two faces of stone or brick (or temporary plank formwork) are raised a little at a time; between them, a layer of mortar is spread and a layer of fist-sized stones is rammed down into it, again and again.
  1. Formwork. For a wall, build two faces — either permanent facings of stone or brick laid in mortar, or temporary planks held by stakes and cross-ties. Wet the formwork so it does not suck water out of the mix. For a foundation, the sides of a trench serve as the mould.
  2. Mortar layer. Spread a layer of pozzolanic or hydraulic mortar 5–10 cm thick between the faces.
  3. Stone layer. Lay a layer of clean, wetted broken stone, brick or gravel — pieces 3–15 cm across (Roman caementa) — into the mortar.
  4. Ram it. Pound it with a heavy rammer until mortar squeezes up between all the stones and no voids or air pockets are left. A properly rammed layer rings dully under the rammer and does not move.
  5. Repeat, layer on layer, no more than 30–60 cm a day of height for lime concrete. Keep the top of each day's work damp and rough, so the next day's layer bonds.
  6. Strike the formwork (remove the planks) after 1–2 weeks for lime-pozzolan concrete, or longer in cold weather. Leave arches and floors propped for at least 4 weeks.

Mixed concrete. For floors, footings and small items you can also mix all the parts first and then place and ram it: roughly 1 lime : 1 pozzolan : 2 sand : 4 gravel by volume, mixed dry, then wetted until it is like stiff, crumbly earth that holds together when squeezed. For portland cement concrete, see Portland Cement.

Curing

Mortar and concrete do not dry hard; they set by chemical reactions that need water and time. If fresh work dries out, the reactions stop and it stays weak and powdery.

  • Keep it damp. Cover fresh work with wet sacking, straw mats or wet sand, and sprinkle it two or three times a day. For lime-pozzolan work, at least 7 days, better 2–4 weeks.
  • Shade it from sun and wind.
  • No frost. Do not lay lime mortar or concrete if the temperature may fall below about 5 °C in the next week or two. Frozen fresh mortar crumbles.
  • Don't load it early. Lime-pozzolan concrete reaches perhaps half its strength in a month and keeps hardening for a year or more. Air-lime mortar is weaker still at first.

How to tell it worked

  • Thumbnail test. After a week, a good lime-pozzolan mortar joint cannot be dented with a thumbnail; after a month it is hard to scratch with an iron nail.
  • Underwater ball. A ball of hydraulic mortar kept under water for 2–4 weeks becomes hard and rings faintly when tapped. Air-lime balls go soft.
  • The bar test. Make three bars of each mix in a wooden mould, about 4 × 4 × 16 cm. Cure them damp for 28 days. Rest each across two supports 10 cm apart and hang a basket from the middle, adding stones until it snaps. Weigh the load. You will not get an engineer's number, but you will learn which of your mixes is strongest — try different pozzolans and ratios and keep the winners. Typical: a good lime-pozzolan bar might take roughly 10–40 kg; an air-lime bar much less.
  • In a wall. Joints stay full and do not powder when rubbed. A cistern lining holds water with the level falling no more than evaporation.

Note Troubleshooting. Mortar cracks in a network of fine lines → too much binder or too much water, or it dried too fast. Use more sand, less water, and keep it damp. Mortar stays soft and powdery for months → air-lime used where air cannot reach, or it dried out before it set. Use a hydraulic mix and cure it damp. Powders when rubbed, even outside → dirty sand (clay or silt in it), or frost got at it. Wash the sand; never build in frost. White crust appears on the wall → salts carried out by water — from salty sand, seawater, or wet ground. Wash the sand; damp-proof the foundations (Foundations and Floors). Cistern leaks → lining too thin or cracked at the corners. Apply in three coats, 2–3 cm in all, with rounded fillets of mortar in every corner, and polish the last coat hard with a smooth stone while it stiffens. Lime-pozzolan ball softens under water → the pozzolan is weak. Grind it finer, use more, or fire clay at a different temperature and test again.

Dangers

Danger Lime and wet mortar burn eyes and skin. Mortar and concrete are strongly alkaline. A splash in the eye can blind: flush with clean water for at least 20 minutes at once. Wet mortar slowly burns skin, often unnoticed until hours later — especially on knees kneeling in it and inside boots. Wear gloves or wrapped hands, cover knees, and wash off splashes. Hot-mixing quicklime spits boiling lime; stand back and shield your face. See Lime.

Danger Fresh concrete and formwork collapse. Wet concrete pushes hard on its formwork — a 1 m high wall of fresh concrete presses about 2.4 tonnes on every square metre of form at the bottom. Tie and brace forms well, fill them slowly in layers, and keep people out of trenches and away from the foot of forms while filling. Never remove props from an arch, vault or floor early.

  • Dust. Sieving lime, volcanic ash and crushed brick makes fine dust; work upwind with a damp cloth over nose and mouth.
  • Strain. Mortar and concrete are heavy: a bucket weighs 20–25 kg. Share the load.

What this unlocks

Mortar lets you build Stone Masonry, brick walls (Bricks), Foundations and Floors, Chimneys, Stoves and Heating and Arches, Vaults and Domes. Hydraulic mortar and concrete build Wells and Cisterns, harbours, bridge piers (Roads and Bridges), Sewers and Wastewater, Pipes, Plumbing and Aqueducts channels and canal locks (Canals and Locks). The search for a stronger, faster hydraulic binder leads straight to Portland Cement, and with iron bars cast inside, to Reinforced Concrete.

How it was first done

People burned lime for plaster in the Near East about 12,000 years ago, and hard lime-plaster floors are found in Neolithic villages there from about 9,000 years ago. Egyptians used gypsum mortar. Builders in Greece and the Near East learned to add crushed pottery to lime to make waterproof plaster for cisterns, and the Nabataeans of Petra used hydraulic lime mortars to line their water channels. The Romans made concrete their main building material from the 2nd century BC: with lime and the volcanic ash of Pozzuoli they built aqueducts, baths, the harbour of Caesarea in Judaea (about 20 BC) out in open sea, and the Pantheon in Rome (about AD 125), whose unreinforced concrete dome, 43 m across, still stands. Recent studies of Roman concrete have found that seawater reacting with volcanic ash grew new crystals inside it over centuries, and that hot-mixed quicklime left lime lumps that can heal cracks. After Rome fell, much of the knowledge was lost. In 1756 the English engineer John Smeaton, building the Eddystone lighthouse on a wave-swept rock, tested limes systematically and found that limestones containing clay make lime that sets under water — the first step toward Portland Cement.

Source: content/entries/earth/mortar-and-concrete.md