◆ Rebuild

Part 15 · Knowledge and Science

Cryogenics and Superconductors

The science and craft of the very cold. How to store liquid nitrogen for months in a metal vacuum vessel, how helium is liquefied at −269 °C, and what happens to some materials when they get that cold — they lose all electrical resistance and push magnets away. How to make a ceramic superconductor that works in liquid nitrogen and float a magnet over it, and, in outline, how niobium–titanium wire and superconducting magnets for scanners and laboratories are made. With the real dangers — cold burns, bursting vessels and silent suffocation.

Difficulty
●●●●●
Time
A week to build a cryostat; a month to make a working ceramic superconductor once you have liquid nitrogen; a year to build a good metal storage dewar; many years and a team for a helium liquefier and superconducting magnets
Steps from zero
40 prerequisites →

You need first

Liquid Air, Nitrogen and the Noble GasesMagnets

This unlocks

Artificial Insemination and Gene Banks
The full path from nothing — 40 steps before this one
  1. Stone Tools
  2. Cordage and Rope
  3. Fire
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Basic Woodworking
  7. Hunting and Trapping
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Salt
  13. Lime
  14. Bricks
  15. Fermentation
  16. Lye and Potash
  17. The Wheel and Axle
  18. Glass
  19. Firebrick and Refractories
  20. Bellows
  21. The Lathe
  22. Gears
  23. Iron (the Bloomery)
  24. Copper Smelting
  25. Laboratory Glassware
  26. Pumps
  27. The Waterwheel
  28. Blacksmithing
  29. The Blast Furnace and Cast Iron
  30. The Battery
  31. Magnets
  32. Steel
  33. The Steam Engine
  34. Bellows to Air Compressors
  35. Electrolysis
  36. Hydrogen, Oxygen and Gases
  37. Machine Tools
  38. Ammonia
  39. Ice and Refrigeration
  40. Liquid Air, Nitrogen and the Noble Gases
  41. Cryogenics and Superconductors

Do them roughly in this order. See it on the tech tree →

Why it matters

The liquid-air machine of Liquid Air, Nitrogen and the Noble Gases gives liquid nitrogen at −196 °C. That cold has uses of its own — storing frozen semen and embryos for livestock breeding (Artificial Insemination and Gene Banks, Embryo Transfer in Livestock) and microbe cultures (Culturing Microbes) for decades, trapping vapours in vacuum systems, freezing warts, shrink-fitting bearings — but only if you can keep it for weeks instead of hours. That needs a good dewar.

Colder still, at −269 °C, helium becomes a liquid, and at those temperatures many metals become superconductors: their electrical resistance vanishes completely. A current started in a ring of superconducting wire runs for years with no battery. Coils of such wire make the strongest steady magnets there are, with almost no power: the magnets of MRI scanners (Ultrasound, CT and MRI), chemical analysis machines, Particle Accelerators (Overview) and some electric power equipment. Since 1987, ceramics have been known that superconduct in plain liquid nitrogen, and one of them can be made in a kiln.

Be honest about the scale. A good nitrogen dewar and a ceramic superconductor are within reach of a workshop that already has liquid air. A helium liquefier and superconducting magnet wire are among the hardest things in this book.

How it works

Temperature near absolute zero

Cold is measured from absolute zero, −273.15 °C, the temperature at which all heat motion stops. On the kelvin scale (K), steps are the same size as degrees Celsius but zero is absolute zero: 0 °C is 273 K, liquid nitrogen boils at 77 K, liquid helium at 4.2 K.

Liquid Boils at Heat to boil 1 litre 1 litre makes this much gas
Nitrogen 77 K, −196 °C 160 kJ: 1 watt of heat leak boils away about 0.5 litre a day about 700 litres
Helium 4.2 K, −269 °C 2.6 kJ: 1 watt boils away about 1.4 litres an hour about 750 litres

Helium is sixty times easier to lose than nitrogen. Everything in helium work is about stopping heat getting in.

Stopping heat

Heat creeps in three ways, and a cryogenic vessel stops each:

  • Through air touching the cold wall: stop it with a vacuum between two walls.
  • As radiation, the invisible glow of warm things: stop it with shiny surfaces — silvering in a glass flask, or many layers of thin aluminium foil in a metal one (multilayer insulation).
  • Through solid parts joining cold to warm: make every support and neck long, thin-walled, and of a poor conductor (thin stainless steel, glass, glass-fibre resin), never copper.

Superconductivity

Cool a superconductor below its critical temperature (Tc) and two things happen:

  1. Its resistance drops to zero — not small, zero. Current flows with no heating and no voltage.
  2. It pushes out magnetic field from inside itself (the Meissner effect). A magnet held over it is repelled. In the ceramic superconductors, some field gets trapped in tiny defects and holds the magnet in place, so it floats firmly and can even hang below.

Superconductivity is destroyed again by too strong a magnetic field (the critical field) or too much current per square millimetre (the critical current). Useful superconductors are those that keep working in strong fields.

Material Tc Notes
Mercury 4.2 K The first discovered, 1911
Lead 7.2 K Easy demonstration in liquid helium; fails in weak fields
Niobium 9.2 K Pure metal; radio-frequency cavities
Niobium–titanium (NbTi) about 9.5 K Ductile alloy, drawn into wire; works to about 9 tesla at 4.2 K; most magnets use it
Niobium–tin (Nb₃Sn) 18 K Brittle; for fields above 10 tesla
YBCO (yttrium barium copper oxide) about 92 K Ceramic; works in liquid nitrogen
BSCCO (bismuth strontium calcium copper oxide) 85–110 K Ceramic; no rare earths needed

(A tesla is a unit of magnetic field: a fridge magnet is about 0.01 T, a strong iron-cored The Electromagnet about 2 T.)

What you need

For You need
Liquid nitrogen A liquid-air machine and column (Liquid Air, Nitrogen and the Noble Gases)
Storage dewar Aluminium or copper sheet, thin stainless steel or glass-fibre tube for the neck, aluminium foil, glass-fibre paper, Activated Charcoal, a diffusion The Vacuum Pump, Welding
Ceramic superconductor Yttrium oxide (Rare Earths, Cerium and Phosphors, from xenotime), barium carbonate (from barite, The Vacuum Tube), copper oxide (from native copper or any copper, Copper Smelting); an agate or porcelain mortar; a steel die and press; a The Kiln or electric furnace reaching 950 °C with a pyrometer; oxygen
Testing A strong small magnet (Permanent Magnets), a thermocouple (Thermocouples and Thermoelectricity), a sensitive voltmeter (Measuring Electricity)
Helium Natural gas rich in helium and a helium plant (Natural Gas and Helium); compressors (Bellows to Air Compressors)
Magnet wire Niobium from columbite, titanium (Titanium), copper, an electron-beam or vacuum arc furnace, Iron and Brass Wire

The liquid nitrogen dewar

Loose cap boiling gas must escape: never seal Long thin neck stainless or glass-fibre, 0.3–0.5 mm wall Outer shell stays at room temperature Vacuum space below 0.0001 mbar Multilayer insulation 20–40 layers of foil and glass paper Liquid nitrogen, −196 °C in an aluminium inner vessel, 25 litres Charcoal getter soaks up the last gas when cold Pinched-off pump tube copper, squeezed shut after pumping 60 cm 38 cm
Fig. 1 A metal storage dewar in cutaway. The inner vessel hangs from a long thin neck inside an outer shell, with a hard vacuum between them, many layers of foil to stop radiated heat, and a packet of charcoal that soaks up the last traces of gas when it gets cold. The loose cap lets boiling gas escape.

The glass Dewar flask of Liquid Air, Nitrogen and the Noble Gases keeps liquid nitrogen for a day or two. A liquid nitrogen dewar of metal holds 10–50 litres for one to six months and does not shatter. It is the vessel farmers use to keep frozen semen.

Sizes for a 25-litre dewar. Inner vessel 28 cm across and 45 cm tall; outer shell 38 cm across and 60 cm tall; neck 5 cm bore and 15–20 cm long, with walls 0.3–0.5 mm thick.

  1. The inner vessel. Weld a cylinder of 1.5–2 mm aluminium or copper sheet with dished ends (Sheet Metal and Rolling, Welding). Test it for leaks under water with air at half a bar, then with a smoke or ammonia test at every seam.
  2. The neck is the main heat path: the whole vessel hangs from it. Use the thinnest tube that will carry the weight — thin stainless steel (Alloy and Stainless Steels) or a tube of glass fibre and resin (Composites: Fibreglass, Carbon Fibre and Honeycomb). A neck 15 cm long instead of 5 cm lets in a third of the heat.
  3. The getter. Fix a flat packet of 50–100 g of Activated Charcoal, wrapped in cloth, to the outside of the inner vessel's base. When the vessel is cold the charcoal soaks up nearly all the gas left in the vacuum space and keeps the vacuum hard for years.
  4. Multilayer insulation. Wrap the inner vessel in 20–40 layers of thin aluminium foil, each separated from the next by one sheet of thin glass-fibre paper or silk, loosely, about 20 layers per centimetre. Pressed tight, the layers touch and lose their value.
  5. Close the outer shell around it, welded to the top of the neck, with a short copper pump-out tube.
  6. Pump out. Connect to a diffusion pump backed by a rotary pump (The Vacuum Pump, High-Vacuum Pumps and Gauges). Warm the whole dewar to 60–80 °C for several days while pumping, to drive water out of the foil and paper. Pump until a gauge reads below about 0.0001 mbar (a ten-millionth of the air's pressure). Then squeeze the copper pump-out tube flat with a heavy pinch tool, which cold-welds it shut, and cut it off beyond the pinch; cap the stub.
  7. Cap: a loose foam or cork plug in the neck, never a seal.

Good or bad. Fill it and weigh it each day. Nitrogen weighs 0.8 kg a litre. A good 25-litre dewar loses 0.2–0.5 litres a day; at first a home-made one may lose 1–2. If it loses 5 litres or more a day, or the outer shell sweats or frosts, the vacuum is poor: find the leak, re-pump, and check the getter. A dewar whose loss creeps up month by month has a slow leak.

For short work, a cryostat — any insulated container where an experiment sits in or over cold liquid — can be a double-walled box of expanded foam or cork, or a glass Dewar flask with a stirrer and a sample holder hanging from a lid on long thin rods. It keeps liquid nitrogen for an afternoon.

Making a ceramic superconductor

This is the most achievable route to superconductivity: a ceramic made like a pottery glaze, which works in liquid nitrogen. Its formula is YBa₂Cu₃O₇: one atom of yttrium, two of barium and three of copper.

Step by step

  1. Weigh for a 6–7 g batch: 1.13 g yttrium oxide (Y₂O₃), 3.95 g barium carbonate (BaCO₃), 2.39 g copper oxide (CuO, black). The proportions matter: weigh to a hundredth of a gram if you can (Balances, Steelyards and Weighing Machines). All three must be pure and dry; heat them first to 300 °C for an hour. Make black copper oxide by heating copper filings in air at a red heat, or by heating copper nitrate (Nitric Acid).
  2. Grind them together in an agate or porcelain mortar for 30 minutes, until the colour is an even grey with no streaks.
  3. First firing. Spread the powder in an alumina or porcelain boat (Firebrick and Refractories) and fire at 930–950 °C for 12–24 hours in air. Barium carbonate gives off carbon dioxide; the powder turns black. Cool, grind again for 20 minutes, and fire again. Two or three rounds give a more complete reaction.
  4. Press pellets. Put 1–2 g of powder in a steel die 13–20 mm across and press it hard — a few tonnes on the plunger, with a screw press or a jack in a frame (Hydraulic Presses and Rams). It comes out a hard black disc 2–4 mm thick.
  5. Sinter the pellets at 930–950 °C for 12–24 hours, in a slow stream of oxygen if you have it (Liquid Air, Nitrogen and the Noble Gases).
  6. Load it with oxygen. This is the step that makes or breaks it. Cool slowly, about 1–2 °C a minute, to 450 °C; hold there for 6–12 hours with oxygen flowing; then cool slowly to room temperature. The ceramic takes up oxygen and its crystals change shape: only the oxygen-rich form superconducts. In air instead of oxygen it may still work, but more weakly.
  7. Store the pellets in a dry, closed jar. Water and damp air slowly spoil them.

Testing it

N S Small strong magnet floats a few mm up gap Pellet, 13–20 mm black YBCO ceramic Liquid nitrogen in a foam dish 70 80 90 100 110 120 130 temperature, kelvin resist- ance 77 K: liquid nitrogen exactly zero normal: about a millivolt Tc about 92 K
Fig. 2 Left: a magnet floats over a pellet of ceramic superconductor cooled in liquid nitrogen. Right: its resistance as it warms — falling to exactly zero below about 90 K.
  • Levitation. Put the pellet in a shallow foam dish and pour liquid nitrogen over it until it stops boiling hard. Lower a small strong magnet onto it with non-metal tweezers — a neodymium magnet works best (Permanent Magnets). It floats a few millimetres above the pellet, steady, and spins freely. As the nitrogen boils off and the pellet warms past about 92 K, the magnet sinks.
  • Resistance (four-probe). Cut or press a bar about 2 × 2 × 15 mm. Attach four fine copper wires with silver paint (silver powder in a varnish, Gold and Silver): the outer two carry about 100 mA from a battery and resistor; the inner two, 5 mm apart, go to a sensitive voltmeter. Measuring voltage on separate wires means the resistance of the contacts does not count. Fix a thermocouple to the bar. Cool it in nitrogen, lift it out, and record voltage and temperature as it warms. Above about 95 K you will read roughly a millivolt; below about 90 K, zero.

Liquid helium

Why it is hard

Helium must be precooled before the throttling trick of the liquid-air machine works at all: above about 40 K, helium squeezed through a valve warms instead of cooling. And at 4 K almost nothing is left to absorb heat; a watt boils away litres an hour.

The helium liquefier, in outline

A helium liquefier of the kind that made liquid helium common after 1946:

  1. Compressor raising pure helium to 15–20 bar, with oil removed completely (Bellows to Air Compressors).
  2. Purifier: a trap of Activated Charcoal cooled in liquid nitrogen, which catches every other gas (air, water, neon). Any impurity freezes solid in the cold heat exchangers and blocks them.
  3. Liquid nitrogen precooling to 77 K.
  4. Counterflow heat exchangers like those of the air machine, but far longer and more efficient.
  5. Two expansion engines: small pistons that let the compressed helium push against a load (a brake or a generator) as it expands. Gas that does work cools sharply, even above 40 K. These bring it to around 10 K.
  6. A final throttle valve at which part of the gas turns to liquid at 4.2 K.

Such a machine makes a few litres of liquid helium an hour. It needs a team that has built liquid-air machines, a supply of helium (Natural Gas and Helium) and a recovery system: every litre that boils off is collected in a gas bag, compressed into cylinders and liquefied again. Helium is too rare to waste.

Storing liquid helium needs a dewar of the kind above with one more layer: a copper shield or second vessel cooled by liquid nitrogen between the helium and the outer wall, so the helium vessel sees only 77 K instead of room temperature.

Superconducting wire and magnets

Vacuum vessel room temperature outside Shield at 77 K cooled by liquid nitrogen Liquid helium, 4.2 K Helium vessel Coil of NbTi wire soaked in epoxy, on a former Persistent switchwith heater Vent / quench pipe to the outdoors Windings in section Field in the bore Current leads Wire, cut across NbTi filaments in copper, 0.5–1 mm across
Fig. 3 A superconducting magnet, simplified. The coil of niobium–titanium wire sits in a bath of liquid helium, inside a nitrogen-cooled shield and a vacuum vessel. A short loop of superconductor with a small heater acts as a switch: opened to charge the magnet, then closed so the current circles for years. Inset: a wire cut across, with thousands of fine superconducting filaments in copper.

Niobium–titanium wire

Niobium comes from columbite, a heavy black ore found with tantalum in granite pegmatites. Separating it from tantalum and refining it to a pure, ductile metal needs fluoride chemistry (Fluorspar and Fluorine Compounds) and melting in vacuum by electron beam or arc — 20th-century industrial methods. Melted with titanium to about 47% titanium by weight, it makes an alloy that draws into wire like copper.

The wire is not solid alloy. Rods of NbTi are packed into a copper can, sealed, hot-extruded, drawn down, cut, restacked and drawn again, until a wire 0.5–1 mm across holds hundreds to thousands of filaments 5–50 micrometres thick, embedded in copper and twisted. Heat treatments between draws create tiny particles in the alloy that pin the magnetic field and raise the current it can carry — about 3,000 amperes per square millimetre of NbTi at 5 tesla and 4.2 K, a thousand times what a copper wire can carry without melting. The copper is essential: if a filament stops superconducting for a moment, the current flows round it through the copper instead of burning it out.

The superconducting magnet

A superconducting magnet is a coil — usually a long solenoid — of this wire, wound tight on a metal former and soaked in epoxy resin so no turn can move. Even a tiny movement under the huge magnetic forces warms the wire enough to stop it superconducting.

  • Charging. Current leads of copper, cooled by the outgoing helium gas, bring current in from a power supply; it is raised slowly over minutes to hours (a large magnet resists any change of current).
  • The persistent switch. A short length of superconductor joins the two ends of the coil, with a small heater on it. With the heater on, that piece is normal and the current flows through the coil from the supply. Turn the heater off: the loop closes, and the current circulates on its own with the supply disconnected. A good magnet loses less than a millionth of its field a day.
  • Quench. If any spot of the coil becomes normal, it heats, the normal zone spreads, and the stored energy — kilojoules in a laboratory magnet, megajoules in a scanner — turns to heat within seconds, boiling off much of the helium. Resistors and diodes across sections of the coil share the heat out so the coil is not damaged, and a quench pipe vents the gas outdoors. New magnets usually quench a few times at rising currents before they reach full field (training).

A 1.5 T whole-body MRI magnet has a bore about 1 m across and holds several hundred to 2,000 litres of liquid helium, topped up rarely.

How to tell it worked

  • Dewar: daily weighing shows a steady loss under 0.5 L a day for a 25 L vessel; the outer shell stays dry and at room temperature.
  • Ceramic: a magnet floats over it in liquid nitrogen and falls when it warms; the four-probe voltage drops sharply to zero near 90 K.
  • Magnet: the field, measured with a Hall probe or the induced voltage in a search coil (Measuring Electricity), stays the same for days in persistent mode.

Note Troubleshooting. Dewar sweats or frosts outside → vacuum lost: leak at a weld or pinch-off, or foil not dried before sealing. Pellet green or brown, not black → wrong proportions or not fired long enough; regrind and refire. Green specks are a known wrong compound. Pellet black but magnet will not float → not enough oxygen: cool more slowly and hold longer at 450 °C in oxygen; or the magnet is too weak. Magnet floats weakly and briefly → pellet too thin or porous; press harder and sinter longer. Resistance falls but not to zero → cracks or a non-superconducting layer; resinter, and check the contacts.

Dangers

Danger Suffocation. Boiling nitrogen and helium contain no oxygen and give no warning: a person in air short of oxygen collapses in a few breaths. One litre of liquid nitrogen becomes 700 litres of gas; a 25-litre dewar spilled in a small room can make the air deadly. A magnet quench can release a thousand cubic metres of helium in a minute. Keep dewars in well-ventilated rooms, never carry them in a closed lift or car cab with people, fit an oxygen alarm where large amounts are kept, and never rush in after a collapsed person without fresh air (Liquid Air, Nitrogen and the Noble Gases).

Danger Bursting. Liquid trapped in a closed space boils and builds pressure until the vessel explodes. Never seal a dewar, flask or pipe holding cryogenic liquid; every space that can trap liquid needs a vent or relief valve. Ice forming in a dewar neck can plug it: clear it with a wooden rod, never by heating with a flame.

  • Cold burns. Liquid nitrogen splashed in the eye blinds; soaked into cloth or trapped in a glove or boot, it freezes flesh deeply. Wear a full face shield, loose dry leather gloves you can shake off, and long trousers over the boots. Treat as in Liquid Air, Nitrogen and the Noble Gases.
  • Liquid oxygen. An open container of liquid nitrogen slowly condenses oxygen from the air; after days it turns faintly blue and becomes a fire and explosion hazard with oil, wood or cloth. Empty old nitrogen safely outdoors.
  • Brittleness. Steel, rubber and most plastics shatter at these temperatures; use copper, aluminium, brass and stainless steel.
  • Barium compounds are poisonous if swallowed or breathed as dust; copper oxide dust is harmful. Grind with a damp cloth over the nose and mouth or under a hood, wash hands, keep food away.
  • Strong magnets. A superconducting magnet pulls tools, gas cylinders and chairs towards it with deadly force, and stops heart pacemakers. Keep all iron away and mark a line round it that no one crosses with metal.

What this unlocks

How it was first done

James Dewar in London invented the vacuum flask in 1892 and liquefied hydrogen in 1898. Heike Kamerlingh Onnes at Leiden in the Netherlands liquefied helium on 10 July 1908, after years building up a cryogenic laboratory, and in 1911, measuring the resistance of frozen mercury with his colleagues, found that it vanished below 4.2 K. Walther Meissner and Robert Ochsenfeld discovered the expulsion of magnetic field in 1933. Samuel Collins at the Massachusetts Institute of Technology built the expansion-engine helium liquefier in 1946, and in a few years liquid helium was available in laboratories worldwide. John Bardeen, Leon Cooper and Robert Schrieffer explained superconductivity in 1957. In the early 1960s high-field superconductors — niobium–tin, shown at Bell Laboratories in 1961 to carry large currents in strong fields, and niobium–titanium soon after — made strong superconducting magnets practical, and the first MRI scanners with them appeared around 1980. In 1986 Georg Bednorz and Alex Müller at IBM in Zurich found a copper-oxide ceramic that superconducted at about 35 K, and in early 1987 Paul Chu, Maw-Kuen Wu and their groups in Houston and Alabama made YBCO, the first superconductor that works above the boiling point of liquid nitrogen.

Source: content/entries/knowledge/superconductors-and-cryogenics.md