◆ Rebuild

Part 3 · Metals

Steel

Iron with a little carbon in it — and the right heat treatment — becomes hard enough to cut iron itself. How to tell steel from iron, how to add carbon, and how to harden and temper an edge by watching its colours.

Difficulty
●●●●●
Time
An hour to harden and temper a blade; one to three days to carburise iron
Steps from zero
12 prerequisites →

You need first

Blacksmithing

This unlocks

AmmoniaPetroleum and RefiningDental Instruments and FillingsMedical InstrumentsCutlery and TablewareRazors, Nail Clippers and Grooming ToolsEngraving, Seals and EtchingPens, Nibs and Writing InstrumentsDrills and BoringMachine ToolsScrews, Nuts and BoltsSpringsThe Blacksmith's ToolingSteel in QuantityAxes, Chisels, Knives and PlanesFiles and SawsHammers, Pliers, Wrenches and ScrewdriversPresses, Punches and DiesScissors, Shears and Folding KnivesIron and Brass Wire
The full path from nothing — 12 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Hides and Leather
  10. Bellows
  11. Iron (the Bloomery)
  12. Blacksmithing
  13. Steel

Do them roughly in this order. See it on the tech tree →

Why it matters

Plain iron from the bloomery is tough but soft. A knife of plain iron dulls on wood; a chisel of plain iron mushrooms when struck. Steel — iron with a small amount of carbon dissolved in it — can be made hard: harder than bronze, hard enough to cut and file plain iron, to hold a razor edge, to throw sparks off flint, and to spring back after bending.

Steel gives you sharp, lasting edges for axes, knives, chisels and The Plough points; it gives you Files and Saws, the tools that shape every other metal part; Springs for traps, locks and clocks; Screws, Nuts and Bolts; and the cutting tools of the The Lathe and Machine Tools. It even makes fire: steel struck on flint is the striker described in Fire.

How it works

Carbon

The amount of carbon decides what the metal can do. The differences are tiny — a few tenths of one percent — but they change everything.

Carbon Name Properties Uses
under 0.1% Wrought or bloom iron Soft, tough, welds easily; does not harden Nails, hinges, chain, bars, tool bodies
0.1–0.3% Mild steel Hardens only a little General ironwork
0.3–0.6% Medium-carbon steel Hardens well, stays tough Axes, hammers, springs, tools that are struck
0.6–1.0% High-carbon (tool) steel Very hard when quenched Knives, wood chisels, punches, springs, files
1.0–1.5% Very high carbon Hardest, but brittle; forges with care Razors, files, engraving tools
2–4% Cast iron Melts at about 1,150–1,200 °C; brittle; cannot be forged Castings: see The Blast Furnace and Cast Iron

Hardening and tempering

When steel is heated to a cherry red (about 750–850 °C), its crystals rearrange into a form that can dissolve the carbon evenly through the metal. If it then cools slowly, the carbon comes back out and the steel is soft. If it is cooled suddenly — plunged into water, brine or oil — the carbon is trapped, and the crystals are locked in a strained, extremely hard state. This is quenching.

Fully quenched steel is hard but as brittle as glass: a quenched blade can shatter if dropped. So it is gently reheated to 200–320 °C, which relaxes some of the strain. This is tempering. It gives up a little hardness for a lot of toughness. The lower the tempering heat, the harder and more brittle; the higher, the softer and tougher.

There is a beautifully simple way to tell when the steel is hot enough to harden: it stops being magnetic. At about 770 °C, iron loses its attraction to a magnet. Touch a lodestone (see Finding and Identifying Ores) or a magnetised bar (see Magnets) to the hot steel; when it no longer sticks, the steel is very close to hardening heat. Give it a moment more in the fire — one colour shade brighter — and quench.

What you need

Item Notes
Forge, anvil, hammer, tongs See Blacksmithing
Iron bars From Iron (the Bloomery) blooms, 3–6 mm thick for carburising
Charcoal powder Fine, 1–3 mm, sieved. Hardwood charcoal is best. See Charcoal.
Charred bone or leather Optional, to mix into the carburising powder
Clay For carburising boxes and seals. See Finding and Preparing Clay.
Quenching liquids Water in a deep bucket (at least 20 L); brine; oil or melted animal fat in a deep clay or metal pot with a lid
Lodestone For the magnet test. See Finding and Identifying Ores.
Sandstone, fine sand To polish the surface before tempering
Grindstone For the spark test and for sharpening: a sandstone wheel on an axle; see The Wheel and Axle

Finding steel in what you have

Your bloom is not all the same. Parts of it, especially near the tuyere where the charcoal was thickest, often picked up enough carbon to be steel. When you break up and forge blooms (see Iron (the Bloomery)), test every piece and keep the steely bits apart. Japanese smiths did exactly this with their bloomery iron, sorting it by how it broke.

The spark test

Hold a piece of metal lightly against a fast-spinning grindstone and watch the sparks in shade. The carbon in steel burns in the hot sparks and makes them burst like tiny fireworks. The more carbon, the more bursts.

Wrought ironlong plain streaks Mild steela few small forks Medium carbonmany forked bursts High carbonshort, bushy stars almost no carbongrindstoneunder 0.3% carbon0.3–0.6% carbonover 0.6% carbon
Fig. 1 Spark test. Plain iron gives long, plain streaks; the more carbon, the more the sparks burst and branch.
  • Wrought iron: long, straight, straw-yellow streaks, almost no bursts; often thickened at the tips.
  • Mild steel: long streaks with a few small forks.
  • Medium-carbon steel: shorter streaks with many bursts that fork.
  • High-carbon steel: short, bright, bushy streaks bursting into star-shaped clusters that burst again.

Test known pieces side by side — a scrap of plain bloom iron and a piece you know hardened well — and compare.

The quench-and-break test

No grindstone? Forge a sample into a small bar about 6 mm square and 8 cm long, and file or chisel a notch halfway along it. Heat it to cherry red and quench it in water. Then:

  • Try to file it. Hardened steel makes a file skate across without biting. Iron files easily.
  • Clamp it and hit it. Iron bends. Steel snaps cleanly like glass at the notch, showing a fine, even, silvery-grey grain. (Wrap it in a rag — the pieces fly.)

Method 1: Carburising (making steel from iron)

If you have no steel, you can put carbon into iron. At a bright cherry to orange heat, carbon from the surrounding charcoal slowly soaks into iron. Done for a short time, this hardens just the surface (case hardening). Done for a long time on thin bars, it turns the whole bar into steel (cementation, which makes blister steel).

Clay boxlid sealed with clay Charcoal powder+ charred bone or leather Iron bars3 cm apart, not touching Witness rodpull out to test BAR, CUT ACROSS steel skiniron core (lighter) Bright cherry to orange, 900–950 °C 2–4 hours for a hard skin · 1–2 days to turn a thin bar to steel
Fig. 2 Carburising box. Iron is packed in charcoal powder inside a sealed clay box and held at a bright cherry-orange heat for hours or days.
  1. Make a box. Form a box or a lidded pot of clay mixed with grog (crushed pottery) and sand, with walls 1.5–2 cm thick, big enough to hold your bars with 3 cm of space around each one. Fire it (see Pottery). For small jobs, an iron tube with its ends clayed shut works too.
  2. Prepare the powder. Sieve fine hardwood charcoal (1–3 mm). Traditionally, smiths mixed in some charred bone, horn, hoof or leather — about one part to four of charcoal — which helps the carbon move into the iron faster.
  3. Pack. Put 3 cm of powder in the bottom, lay in the iron bars (clean, free of scale), and cover them with at least 3 cm more. Bars must not touch each other or the walls. Tamp it down.
  4. Seal. Put on the lid and seal every joint with clay. Air must not get in, or the charcoal will burn away and the iron will scale instead.
  5. Heat. Set the box in a deep charcoal fire, a The Kiln, or the forge, and hold it at a bright cherry to orange heat (900–950 °C) — the whole box evenly glowing.
  6. Time it.
    • Case hardening a finished tool: 2–4 hours gives a hard skin about 0.5 mm deep.
    • Through-carburising a bar 3–5 mm thick: 1 to 2 days of steady heat. Carbon moves in about 1 mm in the first 6–8 hours, then more slowly the deeper it goes. Test by packing a thin "witness" rod alongside the bars, with its end sticking out through the lid. Pull it out after some hours, quench it and break it: a fine silvery grain right through means the bars are done.
  7. Cool slowly in the box, then open it. The bars will be dark grey and may be covered with little blisters.
  8. Even it out. Blister steel is unevenly carburised — high carbon outside, less inside. Cut the bars into short pieces, stack them, forge-weld them together (see Blacksmithing), draw out, fold and weld again. Each fold makes the steel more even. This was called shear steel.

Tip Save your steel. Steel is precious. The old way to make an axe or a knife is to forge the body from plain iron and forge-weld a strip of steel along the edge — the iron body stays tough, the steel edge is hardened. For an axe, split the edge of the iron head with a hot chisel, insert a wedge of steel, and weld it in.

Method 2: Hardening (quenching)

  1. Finish the shape first. Forge it, then grind or file it almost to its final shape, leaving the edge about 1 mm thick. A thin edge overheats and cracks.
  2. Normalise. Heat the whole piece to cherry red and let it cool in still air. Do this three times. It refines the grain and removes forging stresses.
  3. Prepare the quench in a deep container next to the forge:
    • Water — cooling is fast and strong. Good for simple, thick shapes and medium-carbon steel. Warm it to about hand temperature; very cold water cracks more steel.
    • Brine — water with about one cupful of salt (see Salt) per 4 litres. Cools even faster and more evenly than water, because the salt stops a blanket of steam from forming around the steel. For thick high-carbon tools that must be fully hard.
    • Oil or fat — vegetable oil (see Oils and Pressing) or melted animal fat, warmed to about 50 °C (too hot to keep your finger in). Slower and gentler. Best for thin knives, springs and high-carbon steel that cracks in water.
  4. Heat evenly in the heart of a clean charcoal fire, not in the direct blast. Bring it slowly up to cherry red (about 780–830 °C, in shade). Keep the thin edge from overheating by keeping it toward the cooler side of the fire. Check with the lodestone: when it no longer sticks, heat for a few seconds more so the colour is even all over.
  5. Quench. Plunge the piece in vertically, edge or point first, and move it up and down — never side to side, which warps blades. Keep it moving until the hissing stops (water, brine), or until it is cool enough to hold (oil).
  6. Check. Clean a spot with sandstone and try a file on it: it should skate without biting. A hardened edge also scratches glass easily.
  7. Temper at once. Fully hardened steel can crack just sitting on the bench. Do not leave it overnight.

Warning Oil fires. Hot steel in oil makes flames. Use a deep pot with at least 10 cm of oil above the work, keep a tight lid beside it, and if it flares, put the lid on. Never pour water on burning oil.

Method 3: Tempering by colour

  1. Polish. Rub a strip along the blade bright and clean with sandstone and wet sand, so you can see the bare metal.
  2. Heat gently from the back. Lay the spine on a thick bar of iron heated to red, or push the blade into a dish of hot sand on the fire, or hold it high above the coals. The edge must heat last and least.
  3. Watch the colours. As the bright metal heats, a thin film of oxide forms, and its colour shows the temperature exactly: pale straw, straw, brown, purple, blue. Let the colours creep slowly from the back toward the edge.
  4. Quench to stop when the colour you want reaches the edge.
heat the spine; colours creep toward the edge spineedge harder, more brittlesofter, tougher Pale strawStrawBrownPurpleDark blueGrey-blue 220 °C240 °C255 °C275 °C295 °Cover 310 °C razors, files,scrapers knives, woodchisels, drills punches,scissors axes, coldchisels springs,saws too soft:re-harden
Fig. 3 Tempering colours. Watch them run across freshly polished steel and quench when the edge shows the colour for the job.
Colour Temperature Use
Pale straw about 220 °C Razors, scrapers, files, engraving tools — hardest, brittle
Straw about 230–240 °C Knives, wood chisels, drills, plane blades
Brown about 250–260 °C Punches, scissors, axes for light use
Purple about 270–280 °C Axes, cold chisels, tools that are struck hard
Dark blue about 290–300 °C Springs, saws, screwdrivers — tough and springy
Pale blue to grey over 310 °C Too soft for most tools. Re-harden and start again.

For springs, temper the whole piece evenly to blue. For an axe or a chisel, aim for a straw or brown edge with a blue, tougher back. Temper colours appear only on clean metal; old scale or grease hides them.

How to tell it worked

  • The file test. A good edge tempered to straw is just barely touched by a file; the softer spine bites easily.
  • The brass-rod test (once you have brass) or a copper rod: press the edge against the rod at an angle. A good edge bites in and flexes slightly. A too-hard edge chips; a too-soft one flattens.
  • Use. A good knife whittles hardwood all day without rolling or chipping. A good chisel cuts end-grain cleanly and does not dent.
  • Springs return to shape after bending.

Note Troubleshooting. Still soft after quenching → not enough carbon (it was iron — check with the spark test), not hot enough (use the magnet test), or quenched too slowly (try water or brine instead of oil). Cracked in the quench → overheated, too harsh a quench, uneven thickness, or sharp notches. Try oil or warm water; never overheat past bright cherry. Warped → uneven heating, or moved sideways in the quench. Straighten it while still hot from tempering. Edge chips in use → tempered too hard. Re-temper one colour further. Edge rolls or dents → too soft. Harden again and temper less. Grain coarse and sparkly when broken → overheated. Normalise three times and re-harden at a lower heat.

Crucible steel

All the methods above make steel without melting it. In the most advanced pre-industrial process, steel was actually melted. In southern India and Sri Lanka, smiths sealed iron and plant material (wood or leaves) in small clay crucibles and heated them for many hours in a charcoal furnace until the contents melted, making cakes of very high-carbon steel called wootz, famous as the steel of "Damascus" blades. In 1740s England, Benjamin Huntsman melted blister steel in clay crucibles in a coke-fired furnace at about 1,550–1,600 °C, making steel that was uniform all the way through, ideal for springs, clocks and razors. Crucible steel needs crucibles of very heat-resistant clay (see Firebrick and Refractories) and a furnace far hotter than a bloomery. It is a goal for later, once you have Firebrick and Refractories and powered bellows.

Dangers

Danger Quench oil fires and steam. Burning oil can spread across a workshop in seconds. Keep the lid by the pot, work in the open, and keep the pot far from your fuel and bellows. Water and brine quenches can spit boiling water and steam: keep your face away from the bucket.

  • Flying shards. Hardened steel breaks like glass. Wrap test pieces in a rag before breaking them, and never strike a hardened face with a hardened hammer — chips can blind you.
  • Grinding. Sparks and grit from the grindstone fly at the eyes. Turn your face aside and shield it. Keep the wheel wet when sharpening.
  • Carbon monoxide. Carburising boxes and long forge fires make CO. Work in the open.
  • Hot carburising boxes stay dangerously hot for hours. Let them cool in place.

What this unlocks

With hardened and tempered steel you can make Files and Saws — and with files, almost any precise metal part. Steel gives you Springs, better Magnets (hardened steel holds magnetism far longer than soft iron), the cutting tools for the The Lathe and Machine Tools, Screws, Nuts and Bolts, and the cylinders and fittings of the The Steam Engine. Keeping those edges keen is Sharpening and Honing; adding manganese, chromium or tungsten gives the Alloy and Stainless Steels.

How it was first done

Iron Age smiths in the eastern Mediterranean were deliberately carburising and quenching iron by around 1,000 BC. The Greek poet Homer, writing around the 8th century BC, compares the hiss of a burning stake driven into the Cyclops's eye to the hiss of an axe or adze that a smith plunges into cold water to harden it — so quenching was already familiar. Indian wootz steel was being made by several centuries BC and was traded across the ancient world. Japanese swordsmiths sorted steel from iron in their bloomery blooms by breaking and inspecting each piece. In Europe, cementation furnaces made blister steel from the 1600s, Benjamin Huntsman's crucible steel appeared in Sheffield around 1740, and Henry Bessemer's converter made steel cheap enough for railways in 1856 (see Steel in Quantity).

Source: content/entries/metals/steel.md