Alum and Alumina

Alum is a clear, sour-sweet salt of aluminium that bites dyes into cloth, stops shaving cuts, hardens paper and clears muddy water. Made from burnt shale, volcanic alunite or plain white clay with sulfuric acid, it is also the easiest road to pure alumina, a white powder that polishes, survives furnace heat and becomes aluminium metal.

Difficulty
●●●●●
Time
An afternoon to digest clay and a few days to crystallise alum; a day to precipitate and calcine alumina; months for the old shale-heap method
Steps from zero
10 prerequisites →

You need first

Sulfuric AcidFinding and Preparing Clay

This unlocks

—
The full path from nothing — 10 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Sulfur
  4. Pottery
  5. The Kiln
  6. Lime
  7. Lye and Potash
  8. Glass
  9. Saltpeter
  10. Sulfuric Acid
  11. Alum and Alumina

Do them roughly in this order. See it on the tech tree →

Why it matters

Alum is one of the oldest bought-and-sold chemicals in the world. For two thousand years dyers paid fortunes for it, because it makes madder red and weld yellow stay in cloth (Dyes and Mordants). It does many other small jobs too:

  • It stops bleeding from shaving nicks and small cuts: rub a wet styptic block on them.
  • It sizes paper. With rosin soap it lets a paper mill make writing paper in one step, without tub-sizing every sheet in glue (Paper).
  • It clears muddy water for a whole town (Water Treatment for a Town).
  • It taws skins into soft white leather, makes lake pigments from plant dyes (Pigments, Paints and Varnish), and hardens gelatin.

Alum is also the cleanest road to alumina (aluminium oxide). Calcined hot, alumina is a white powder nearly as hard as sapphire. It polishes steel and glass, lines furnaces (Firebrick and Refractories), grows rubies (Synthetic Gems), and is the raw material for Aluminium metal. Calcined gently, it becomes a thirsty, porous grit that dries gases and pulls fluoride out of drinking water (Fluorspar and Fluorine Compounds).

The Dyes and Mordants chapter gives a short recipe for alum from shale and alunite. This chapter covers the whole family. It shows how to make alum from ordinary white clay, how to purify it, how to use it, and how to turn it into alumina.

How it works

Aluminium is in every clay, but there it is locked to silica, and water cannot get it out. Hot sulfuric acid pulls the aluminium out of clay as aluminium sulfate. Aluminium sulfate dissolves very well in water but is reluctant to crystallise. Add a potassium salt (potash) or an ammonium salt (from stale urine or gasworks liquor), and it forms a double salt: alum. Alum crystallises easily into big clear eight-sided crystals.

Name What it is Notes
Potash alum Potassium aluminium sulfate, with 12 parts of water locked in the crystal The classic alum
Ammonium alum Ammonium aluminium sulfate, also with 12 waters Almost identical; it burns away completely to pure alumina
Papermaker's alum Aluminium sulfate alone Cheaper; sold as a lumpy solid or strong syrup; used for paper and water
Burnt alum Alum dried above 200 °C Light white powder, strongly drying

Two facts make alum easy to purify:

  1. It dissolves far better hot than cold. About 11 g of potash alum dissolves in 100 ml of water at 20 °C. Near boiling, more than its own weight dissolves. So a hot, strong solution, cooled, drops most of its alum as crystals and leaves dirt such as iron in the liquid.
  2. Iron is the enemy. Shale and clay always contain iron. Iron spoils bright dyes, browns paper and colours alumina. Each recrystallisation removes most of what is left.

Alumina comes from alum in two steps. First add an alkali, which throws down white jelly-like aluminium hydroxide. Then calcine it, which means heating it hard in air. The heat decides what you get:

Calcining heat Product Character
400–600 °C (dull red just visible in the dark) Activated alumina Soft, chalky, full of tiny pores; soaks up water and fluoride
1,200–1,300 °C (yellow-white) for several hours Alpha alumina (artificial corundum) Dense, hard grains (hardness 9), scratch quartz; does not melt below 2,050 °C
Making alum 1 Calcine claydull red, 600–750 °C2–3 hours, then grind 2 Digest in acidclay + dilute sulfuric acidnear boiling, 3–4 hours 3 Filter, add potashor ammonium sulfate or urine dissolve hot, cool again4 Crystalliseeight-sided alum crystalsrecrystallise 2–4 times pure alum Making alumina 5 Add soda ashwhite jelly falls out 6 Wash 6–8 timessettle and pour off 7 Calcinethe heat decides 450–550 °Cactivated alumina:soft, porous, drinks water 1,200–1,300 °Calpha alumina: hard,scratches glass, polishes
Fig. 1 From clay to alum to alumina. Hot sulfuric acid pulls aluminium out of calcined clay; potash or urine turns it into alum, which is purified by crystallising it again and again. Alkali throws down aluminium hydroxide, and the calcining heat decides whether it becomes soft, porous activated alumina or hard alpha alumina.

What you need

For about 200 g of alum from clay:

Item Amount Notes
White clay or kaolin, calcined 100 g The whiter the better (Finding and Preparing Clay)
Concentrated Sulfuric Acid 70 ml (130 g) Or about 400 ml of the weaker chamber acid
Potassium sulfate 65 g From potash and sulfuric acid, or the salt left over from making Nitric Acid. Or 50 g ammonium sulfate, or 300–500 ml of stale urine
Glazed stoneware or lead pan, 1.5 litres Acid eats iron and unglazed pottery
Wooden or glass stirrer
Cloth and a bed of clean sand in a funnel For filtering
Shallow glazed dishes or a wooden tub For crystallising

For alumina, add soda ash (Soda Ash and Baking Soda) or ammonia solution (Ammonia), plenty of clean rainwater, and a clay crucible and The Kiln.

Where to find it

  • Alum shale. Dark grey to black, papery shale, speckled with brassy pyrite. Where it weathers it grows white, fluffy, sour-tasting crusts, and streams below it run clear but taste inky. The famous works at Whitby in Yorkshire burned about 50 tonnes of shale for every tonne of alum (Rocks and Minerals).
  • Alunite (alum stone). A whitish, pinkish or grey, fine-grained rock in old volcanic districts, where hot acid steam has rotted lava. It feels harsh and slightly sandy and does not fizz in acid. The papal mines at Tolfa near Rome worked it for four centuries.
  • Kaolin and white clay. These are everywhere, and they are the most reliable source. Kaolin is about 35–40 % alumina (Finding and Preparing Clay). Pick the whitest. Clay that fires red is rich in iron and gives yellowish alum.
  • Bauxite. Red, pink or cream earthy rock of hot climates, rich in alumina (Aluminium). It dissolves in hot sulfuric acid even more easily than clay, but brings more iron.
  • Natural alum crusts. These grow on burnt or weathering shale, in volcanic vents and in some dry caves. Taste a crumb: alum is first sweetish, then fiercely drying, as if your mouth were shrinking.

Method 1: Alum from white clay

  1. Calcine the clay. Raw clay resists acid. Crumble dry clay into walnut-sized lumps and heat it at a dull red, 600–750 °C, for 2–3 hours, for example in a The Kiln beside pots. Do not go to bright red, or it turns back into something acid cannot touch. It comes out pale pink-grey and lighter. Grind it to flour.
  2. Make the acid bath. Put 250 ml of water in the glazed pan, then pour in the 70 ml of concentrated acid slowly, stirring. Always acid into water, never water into acid. It gets hot.
  3. Digest. Stir in the 100 g of clay and keep the pan just below boiling for 3–4 hours, stirring now and then and topping up the water as it steams away. The grey mud grows thick and pasty as aluminium sulfate forms.
  4. Dilute and settle. Add 300 ml of hot water, stir, and let the silica settle for an hour. Pour the cloudy-clear liquid through cloth, then through sand. Wash the residue once more with 100 ml of hot water and add that too. The residue is fine silica, which is useful in Glazes and polishing.
  5. Add the potassium. Dissolve the 65 g of potassium sulfate in the least amount of hot water and stir it into the hot liquid. With urine, add it and boil for 10 minutes; it smells strongly.
  6. Concentrate. Boil the liquid down until a drop on a cold stone grows small crystals within a minute.
  7. Crystallise. Pour it into a clean dish, cover it with a cloth, and leave it in a cool place for 1–3 days. Clear crystals grow on the bottom and sides. Pour off the liquid and boil it down again for a second crop.
  8. Recrystallise. Dissolve the crystals in the least amount of boiling water, about 1 ml for each gram, then let them cool slowly. Do this two or three times for dyeing or medicine, and four times for alumina that must be pure white.

Yield: 100 g of good calcined kaolin gives 150–250 g of alum, against a theoretical 360 g.

The old ways, from shale and alunite

Shale. Heap the broken shale over brushwood and let it smoulder for months. The pyrite burns to sulfuric acid inside the heap and attacks the clay. Leach the red, burnt shale with water, as you leach ash for Lye and Potash, boil it down, add potash or urine, and crystallise (Dyes and Mordants gives the details). This route needs no bought acid, but a great deal of shale, fuel and time.

Alunite already contains potassium and aluminium sulfate. Roast it at a dull red for a few hours, then heap it and keep it wet for several weeks until it falls to mud. Leach it and crystallise.

Ammonium alum

Use 50 g of ammonium sulfate in step 5 instead of potassium sulfate. Ammonium sulfate comes from ammonia and sulfuric acid (Ammonia, Chemical Fertilisers) or from gasworks liquor (Coal and Coke). The crystals look the same. Choose ammonium alum when you want alumina, because when calcined it leaves nothing but alumina. Potash alum leaves potassium sulfate behind.

Using alum

Styptic block and styptic pencil

A styptic stops bleeding. Alum makes the proteins in blood and skin clot and tightens the tiny vessels of a shaving nick. Use it only on small cuts. A deep wound needs pressure and Wound Care and Antiseptics.

The block. The simplest is a single large crystal. Hang a small, clear seed crystal on a thread in a jar of alum solution that was saturated hot and allowed to cool. Keep it covered at an even temperature. Each week, pour off the liquid, add more alum, warm it to dissolve, cool it, and hang the crystal back. In 2–3 weeks it grows to the size of a hen's egg. Grind one face flat on a wet stone.

Grown block Alum crystalon a thread, froma small seedSaturatedsolution; feedweekly, 2–3 weeks one face ground flat on a wet stone Cast pencil Melted alum, 92 °Cin its own crystal waterBoiling water bathnever a bare flame Clay plugstops one endMouldgreased reed or brass tube, 8–10 mmPencil8–10 cm, paper-wrapped
Fig. 2 The styptic block and styptic pencil. Left: a large alum crystal grown on a thread from a seed, then ground flat on one face. Right: alum melted in its own crystal water at about 92 °C is poured into a greased reed or brass tube, cooled, and pushed out as a pencil.

The cast block and pencil. Alum crystals melt in their own crystal water at about 92 °C, just below boiling.

  1. Put clean crystals in a glazed cup and stand the cup in a pan of boiling water. They melt to a clear, thick liquid.
  2. Never heat it over a bare flame. Above about 100 °C it loses its water, froths and sets into a useless white sponge of burnt alum.
  3. Pour the liquid into moulds greased with a little fat. Use reed, bamboo or brass tubes 8–10 mm across and 8–10 cm long for pencils, stopped at one end with clay. Use a small wooden box about 5 × 3 × 2 cm for a block.
  4. Let it set for an hour, then push the pencil out with a stick.
  5. Wrap the top half of a pencil in paper. To use it, wet the tip, press it on the cut for a few seconds, rinse it and let it dry. It stings briefly.

Good or bad: a good block is hard, clear to milky-white and smooth, and it does not crumble in the hand. A chalky, crumbling block was overheated. A yellow one holds iron; recrystallise it.

Burnt alum. Heat crystals in an iron or clay pan at about 200–250 °C until they puff up into a light, white, dry mass, then grind it. Dusted on, it stops oozing small wounds and dries mouth ulcers. Keep it in a closed jar.

Mordant, tawing and lake pigments

  • Mordant: 10–12 % of the wool's weight, or 15–20 % for linen and cotton after tannin. See Dyes and Mordants.
  • Tawing (white leather). For each kilogram of wet, dehaired and limed-then-washed skin (Hides and Leather), dissolve 100–150 g of alum and 50–75 g of salt in 2 litres of warm water. Soak the skin for 3–7 days, turning it daily. Dry it slowly, working and stretching it as it dries. Tawed leather is soft, white and strong, good for gloves, laces and bookbinding (Leatherwork and Harness-Making, Bookbinding). But it is not waterproof, and soaking washes the alum out.
  • Lake pigments. Boil a dye such as madder, weld or brazilwood, stir in alum solution, then add soda solution a little at a time. The aluminium hydroxide falls out and carries the dye with it as a coloured powder. Wash it, dry it and grind it into oil or gum for paint (Pigments, Paints and Varnish).

Sizing paper with rosin and alum

Gelatin sizing (Paper) treats one sheet at a time. Rosin and alum size the pulp itself, before sheets are formed. This is how most paper was made from the 1830s on.

  1. Rosin soap. Boil 100 g of pine rosin (Tar, Pitch and Glue) with 15–20 g of soda ash in 1 litre of water for 2–3 hours, stirring, until it forms a smooth, brown, soapy liquid.
  2. Stir this into the beaten pulp to give 1–2 % rosin on the dry weight of fibre.
  3. Then add papermaker's alum (aluminium sulfate) or ordinary alum solution, 2–4 % of the fibre weight, until the water just turns blue litmus red (Acids, Bases and Testing). The rosin falls onto the fibres as a water-repelling coat.
  4. Make sheets as usual. Test them with a line of Ink: it should stay sharp.

Warning Rosin-alum paper is acid paper. The acid it carries slowly eats the cellulose. Books made this way between about 1850 and 1980 are now yellow and brittle. For records that must last centuries (Libraries and Preserving Knowledge), size with gelatin, add only a little alum to harden it (0.5–1 % of the gelatin solution), and store the books dry.

Clearing water

A dose of 10–50 mg of alum per litre, found by a jar test, makes the clay in muddy water clump into flakes that settle. Water Treatment for a Town gives the full method.

Method 2: Alumina powder

  1. Dissolve 100 g of pure, recrystallised alum in 1 litre of hot rainwater.
  2. Precipitate. Stir in a solution of 35 g of soda ash in 300 ml of water, a little at a time. It fizzes. Or use ammonia solution, which leaves fewer salts behind. Stop when a drop of the liquid just turns red litmus blue. Do not add caustic lye: excess lye dissolves the aluminium hydroxide again. A white, jelly-like mass forms.
  3. Age it. Keep it warm, about 60 °C, for a few hours or overnight. The jelly becomes more granular and easier to wash.
  4. Wash it thoroughly. Let it settle, pour off the liquid, and stir in fresh hot water. Repeat 6–8 times, until a drop of the wash water evaporated on clean glass leaves no ring. Washing is slow but essential: left-over salts make alumina sinter and glaze.
  5. Dry it on a clay plate. It shrinks to hard, glassy-white lumps. 100 g of alum gives about 11 g of alumina in the end.
  6. Calcine. Use a clean clay or alumina dish, covered.
    • For activated alumina, heat it at 450–550 °C, a dull red just visible in a dark room, for 3–4 hours.
    • For polishing and refractory alumina, heat it at 1,200–1,300 °C, yellow-white, for 4–6 hours in the hottest part of a good kiln.
  7. Grind and grade. Grind the hard alumina wet in an agate or porcelain mortar, never in iron. Then sort it into grades by letting it settle in water (Abrasives and Grinding Stones). Wash the activated grade and keep it in a closed jar.

Shortcut with ammonium alum. Heat ammonium alum slowly in a clay dish. It melts, swells into a huge white sponge and gives off choking fumes of ammonia and sulfur trioxide. Finish at 1,000–1,100 °C (yellow heat) for 2–3 hours: only fine, fluffy, pure alumina is left. Do this outdoors, upwind. This is the powder used for rubies (Synthetic Gems).

Uses of alumina powder

  • Polishing. Levigated alpha alumina, as fine as flour, on a cloth or leather lap with water, gives a mirror finish on steel, brass, gem stones and microscope samples of metal (Gem Cutting and Lapidary, Precision Grinding). Use coarse grades, 20–50 µm, to grind glass, and fine grades, 1 µm and below, for the final polish. For glass, cerium oxide works even faster (Rare Earths, Cerium and Phosphors).
  • Sandblasting grit. Coarse grains cut glass for etched patterns without the lung danger of quartz sand (Fluorspar and Fluorine Compounds).
  • Drying gases and liquids. A jar of activated alumina takes up about a fifth of its own weight of water from damp air. Dry it again at 200–300 °C and reuse it.
  • Removing fluoride from well water (Fluorspar and Fluorine Compounds).
  • Chromatography. Activated alumina packed in a glass tube is one of the standard column packings for separating mixtures (Chromatography).
  • Aluminium metal in the Aluminium cell, which needs kilograms. For that, alumina from bauxite by the Bayer process (Aluminium) is cheaper than from alum.
  • Fused alumina. Melted in an The Electric Arc Furnace from bauxite, then crushed, it becomes the brown grit of most grinding wheels.

The alumina crucible

For melting platinum, rare-earth metals or very hot glasses, or firing phosphors for lamps (Light-Emitting Diodes), clay crucibles are not enough (Firebrick and Refractories).

  1. Mix 90 parts of calcined alpha alumina, ground fine, with 10 parts of white ball clay or kaolin as a binder, and water to a stiff dough.
  2. Press it into a greased plaster or wooden mould, or turn it on a The Potter's Wheel like a small cup. A typical crucible is 4–6 cm across and 5–8 cm tall, with walls 4–6 mm thick.
  3. Dry it for a week.
  4. Fire it as hot as your kiln will go, at least 1,400 °C, and better 1,600 °C in an oxygen-fed or electric furnace.

A well-fired crucible rings when tapped, is white or cream right through, and does not take up ink. A crumbly crucible was fired too cool.

How to tell it worked

  • Alum: clear, eight-sided crystals like two pyramids base to base. They taste sweetish, then puckering. A crumb heated on a clay sherd froths into a white sponge.
  • Iron-free: dissolve a little alum in water and add a few drops of oak-gall tea (crushed oak galls steeped in water). It should stay clear, not turn grey-black. If you have yellow prussiate (Prussian Blue and the Prussiates), even a trace of iron turns it blue.
  • Alpha alumina: rub it between two pieces of glass. It scratches the glass deeply and grits like sand. Activated alumina is soft and barely marks glass. Dropped into water, the activated form gives off a stream of tiny bubbles and grows slightly warm as it drinks.

Note Troubleshooting. Little alum from the clay → the clay was not calcined, was calcined too hot (bright red), or the acid was too weak. Calcine at dull red and digest longer. Liquid will not crystallise → not enough potassium or ammonium. Add a little more, and boil it down further. Yellow or brownish crystals → iron. Recrystallise once or twice more, and use whiter clay. Alumina jelly will not wash or filter → it was precipitated cold and fast. Age it warm overnight, and wash by settling, not filtering. Calcined alumina is glassy or lumpy → salts were left in. Wash better before calcining.

Dangers

Danger Concentrated sulfuric acid blinds and burns deeply, and adding water to it makes it boil and spit. Wear eye protection, pour acid into water, and keep a bucket of water at hand (Sulfuric Acid).

  • Fumes. Calcining ammonium alum and digesting clay give off choking ammonia, sulfur trioxide and acid mist. Work outdoors, upwind.
  • Alum itself is fairly safe in small amounts, but a large swallowed dose (tens of grams) burns the stomach and has killed children. Store it like other chemicals (Emergencies).
  • Dust. Fine alumina and calcined clay dust irritate the lungs. Grind wet.
  • Melted alum is at 92 °C and sticks to skin. Pour it carefully.

What this unlocks

Alum gives you bright dyes and mordants (Dyes and Mordants), white leather, lake pigments, sized paper, styptics for the The First Aid Kit and barber's kit (Razors, Nail Clippers and Grooming Tools), and clear water for towns. Alumina leads to Aluminium, Synthetic Gems and jewel bearings, high-temperature crucibles and furnace linings (Firebrick and Refractories), grinding wheels (Precision Grinding), and the porous alumina used for drying, catalysis and fluoride removal. The same oxide, grown electrically as a thin hard skin on aluminium metal, is Anodising Aluminium and Titanium.

How it was first done

Natural alum was dug in Egypt and on the Greek islands in ancient times, and Pliny described its use in dyeing and medicine. In medieval Europe the best alum came from Phocaea in Asia Minor, traded by the Genoese, until the Ottoman conquest cut it off. In 1461–1462 Giovanni da Castro found alunite at Tolfa, and the papacy held a near-monopoly on it for generations. Alum works on the Yorkshire coast began around 1600 and ran until 1871, burning mountains of shale and buying ship-loads of urine from London. In 1797 Jean-Antoine Chaptal in France described making alum from clay and sulfuric acid. In 1807 Moritz Illig in Germany published rosin-alum sizing for paper. Pure alumina became an industry in the 1890s, for the new Aluminium smelters.