◆ Rebuild

Part 3 · Metals

Alloy and Stainless Steels

A few percent of manganese, nickel, chromium, tungsten or vanadium turns ordinary steel into tool steel that cuts while red-hot, springs that never tire, tough gears and shafts, wear plates that harden as they are hammered, and stainless steel that does not rust. How to find the ores, make the additions and heat-treat the result.

Difficulty
●●●●●
Time
Months to find and smelt the ores into ferroalloys; a single melt once you have them
Steps from zero
27 prerequisites →

You need first

Steel in QuantityThe Electric Arc Furnace

This unlocks

Transformer Steel, Ferrite and Magnetic ShieldingForge Shops and Heat TreatmentJet Engines

Objects made here

ferroalloyspring steel
The full path from nothing — 27 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. The Kiln
  10. Pottery
  11. Hides and Leather
  12. Bricks
  13. The Wheel and Axle
  14. Firebrick and Refractories
  15. Bellows
  16. Gears
  17. Iron (the Bloomery)
  18. Copper Smelting
  19. The Waterwheel
  20. The Blast Furnace and Cast Iron
  21. Blacksmithing
  22. Magnets
  23. Steel
  24. Copper Wire
  25. Steel in Quantity
  26. The Generator
  27. The Electric Arc Furnace
  28. Alloy and Stainless Steels

Do them roughly in this order. See it on the tech tree →

Why it matters

Plain carbon steel (see Steel) is wonderful, but it has limits. It loses its hardness above about 200–250 °C, so a lathe tool cutting fast softens in its own heat. Thick pieces harden only on the surface. It must be quenched violently in water, which cracks complicated shapes. And it rusts.

Adding small amounts of other metals fixes each of these:

  • Tool steels that stay hard even when red-hot, letting Machine Tools cut five to ten times faster.
  • Spring steels for vehicles, clocks and machines that bend millions of times without tiring (Springs).
  • Tough steels for shafts, gears, axles and crankshafts of the The Internal Combustion Engine engine and the The Motor Vehicle.
  • Bearing steels that stay hard and smooth for years (Bearings and Lubrication).
  • Manganese steel that gets harder the more it is battered, for rock crushers and rail crossings.
  • Stainless steel for kitchens, surgical instruments (Sterilising Instruments and Dressings), food and chemical vessels.
  • Special steels: silicon steel for The Transformer cores, and invar, which barely expands with heat, for clock pendulums and measuring tapes.

This is a chapter for a society that already has Steel in Quantity, an The Electric Arc Furnace, and some chemistry. Each alloying metal is a separate search for an ore and a separate smelting job. Start with manganese — it is the most common, the easiest, and you need it for all steelmaking anyway — then chromium, then the others.

How it works

Alloying elements do four main things:

  1. They make steel harden deeper and more gently. In plain steel, the change to hard steel during quenching must happen within about a second, so only the outside of a thick bar cools fast enough. Manganese, chromium, nickel and molybdenum slow this change down. The steel then hardens right through, even when quenched in oil, or for some steels just in air — which also means far less cracking and warping. This is called hardenability.
  2. They form hard carbides. Chromium, tungsten, vanadium and molybdenum join with carbon into tiny particles much harder than steel itself. These resist wear and, crucially, do not soften when hot. A high-speed tool keeps its edge at a dull red heat (about 550–600 °C).
  3. They toughen the steel. Nickel and small amounts of vanadium make the grain fine and the steel tough, so it bends rather than snaps — especially in the cold.
  4. They protect against rust. With at least 11–12% chromium, steel covers itself with an invisible film of chromium oxide only a few atoms thick. The film is tight and self-healing: scratch it and it re-forms within moments. This is stainless steel.
Hardening depth 5 cm bars, quenched and cut across Rust and the stainless film the surface, magnified Plain carbon steel water quench: hard skin 2–4 mm, soft core Alloy steel oil quench: hard right through, less cracking hardened stayed soft air and water air and water Plain steel rust is loose and flaky; air gets through, rust eats deeper and deeper Stainless, 12%+ Cr a chromium oxide film a few atoms thick seals it; a scratch heals in moments scratch
Fig. 1 Left: a quenched bar of plain carbon steel hardens only in a thin skin, but an alloy steel bar of the same size hardens right through. Right: rust on plain steel is loose and flaky and lets air in, while stainless steel is sealed by a thin chromium oxide film that heals itself when scratched.

The elements

Element Typical amount What it does Ore
Manganese (Mn) 0.3–1% in all steel; 12–14% in Hadfield steel Removes oxygen and sulfur; deeper hardening; in large amounts makes steel tough and work-hardening Pyrolusite
Silicon (Si) 0.2–0.4%; 1.5–2% in springs; 3–4% in electrical steel Deoxidiser; spring toughness; reduces losses in transformer iron Quartz (via ferrosilicon)
Nickel (Ni) 1–5%; 8–10% in stainless; 36% in invar Toughness, especially in cold; with chromium, keeps stainless non-magnetic Garnierite, pentlandite
Chromium (Cr) 0.5–1.5% in tool and bearing steels; 12–18% in stainless Deep hardening, wear resistance; rust resistance above 11% Chromite
Tungsten (W) 1–2% in tool steel; 14–18% in high-speed steel Keeps hardness when hot Wolframite
Vanadium (V) 0.1–0.25%; 1–2% in high-speed steel Fine grain, toughness; very hard carbides Vanadinite; some iron ores
Molybdenum (Mo) 0.2–0.5%; up to 9% in some high-speed steels Deep hardening; can replace much of the tungsten Molybdenite

Useful alloy steels

Steel Composition (approx.) Hardening Uses
Silicon–manganese spring steel 0.55–0.6% C, 1.5–2% Si, 0.7–1% Mn Oil from 870 °C; temper 450–500 °C Leaf and coil springs
Chromium bearing steel 1% C, 1.5% Cr Oil from 840 °C; temper 150–180 °C Balls, rollers, races
Nickel–chromium steel 0.3–0.4% C, 3% Ni, 1% Cr Oil from 830 °C; temper 550–650 °C Shafts, gears, axles, crankshafts
Oil-hardening tool steel 0.9% C, 1–1.2% Mn, 0.5% Cr, 0.5% W Oil from 800–820 °C; temper 180–250 °C Dies, taps, gauges, punches
High-speed steel ("18-4-1") 0.7–0.8% C, 18% W, 4% Cr, 1% V Preheat to 850 °C, then quickly to 1,260–1,290 °C (white heat); oil or air; temper twice at 550–570 °C Lathe and drill tools
Hadfield manganese steel 1–1.4% C, 12–14% Mn Heat to 1,000–1,050 °C, quench in water (this softens it and makes it tough) Crusher jaws, digger teeth, rail crossings
Martensitic stainless 12–14% Cr, 0.15–0.4% C Oil or air from 950–1,000 °C; temper 150–300 °C Knives, scissors, surgical tools, valves
Austenitic stainless ("18/8") 18% Cr, 8–10% Ni, under 0.08% C Does not harden; soften by quenching from 1,050 °C Pans, food and chemical vessels
Invar 36% Ni, very low carbon — Pendulums, measuring tapes (The Mechanical Clock, Measurement from Scratch)
Electrical (silicon) steel 3–4% Si, very low carbon Anneal slowly The Transformer and The Electric Motor cores

Where to find it

Pyrolusite (manganese) sooty black, blackens fingers; fern-like black growths on rock Chromite (chromium) heavy black grains, brown streak, in dark green serpentine rock Garnierite (nickel) apple-green crusts in red soil over serpentine; hot wet lands Wolframite (tungsten) black-brown blades, one flat cleavage; very heavy; with tin Vanadinite (vanadium) small red six-sided crystals in weathered lead deposits Molybdenite (molybdenum) soft lead-grey flakes like graphite; greenish streak on glazed pottery
Fig. 2 Ores of the alloying metals. Most are heavy, dark minerals; the tests that tell them apart are the streak, the weight, the magnet and the colour they give a borax bead.
  • Pyrolusite (manganese dioxide) — soft, sooty-black masses and crusts that blacken your fingers; black streak; often as fern-like black "dendrites" on rock surfaces, and as nodules and layers in sedimentary rocks and in the weathered crusts above them. A harder, smooth, black kidney-shaped form is psilomelane. A pink, glassy mineral that fizzes in warm acid is rhodochrosite, manganese carbonate — also a good ore. See Finding and Identifying Ores.
  • Chromite — black, heavy, slightly greasy-metallic grains or masses with a dark brown streak (magnetite's is black), weakly magnetic. Found only in dark green to black serpentine and other very dark, heavy rocks from deep in the Earth (ultramafic rocks), and as black grains in sands below them.
  • Garnierite — a bright apple-green to emerald-green soft crust or earthy mass in the deeply weathered red soils over serpentine, in hot, wet countries. A good ore for ferronickel. Pentlandite, nickel–iron sulfide, is bronze-yellow and occurs mixed with magnetic, bronzy pyrrhotite; this is the world's other main nickel source. Iron meteorites contain 5–10% nickel.
  • Wolframite — very heavy (nearly three times the weight of ordinary stone), dark brown to black, with one perfect flat cleavage and a submetallic shine; dark brown streak. It is found in quartz veins in and around granite, usually with tin ore (see Tin and Pewter). Scheelite, the other tungsten ore, is pale, glassy, and just as heavy.
  • Vanadinite — bright red to orange, small six-sided crystals in the weathered parts of lead deposits (see Lead). Some magnetite ores also carry vanadium: smelting them in a blast furnace concentrates it into the slag, from which it can be recovered.
  • Molybdenite — soft, flaky, lead-grey with a bluish tinge; looks like graphite but is heavier, bluer, and leaves a greenish-grey streak on glazed pottery. In quartz veins and granites.

The borax bead test

The classic field test for these metals needs only borax (see Borax and Boric Acid), a loop of iron or platinum wire, and a hot flame — ideally a blowpipe on a candle or spirit lamp.

  1. Heat the wire loop, dip it in powdered borax, and melt it into a clear glassy bead.
  2. Touch the hot bead to a speck of powdered mineral and melt it in again.
  3. Look at the colour when cool, in the outer (oxidising) part of the flame:
    • Manganese: violet to amethyst.
    • Chromium: emerald green.
    • Nickel: brown to reddish-brown.
    • Cobalt: deep blue (a useful pigment metal, often found with nickel).
    • Iron: yellow to brownish when hot, pale when cold.

A second test for manganese and chromium: melt a little powdered ore with soda ash and saltpeter (see Soda Ash and Baking Soda and Saltpeter) on a piece of broken pottery. Manganese gives a blue-green mass; chromium gives a yellow one that dissolves into a yellow solution in water. The yellow chromium salt is poisonous: handle it with care and wash your hands.

Making the ferroalloys

You do not add pure metals to steel. You add a ferroalloy — the alloying metal smelted together with iron and carbon — which is easier to make and dissolves quickly in a steel bath.

  • Spiegeleisen and ferromanganese. Mixed with iron ore and smelted in a blast furnace (see The Blast Furnace and Cast Iron), manganese ore gives spiegeleisen (15–30% manganese). With rich ore in a hotter furnace you get ferromanganese (70–80%). This was the 19th-century route and needs no electricity. In an arc furnace it is easier (see The Electric Arc Furnace).
  • Ferrochrome. Chromite smelted with coke in a submerged-arc furnace gives high-carbon ferrochrome (about 60% chromium, 6–8% carbon). Good for tool and bearing steels — but stainless steel must be low in carbon, because carbon locks up chromium. For stainless you need low-carbon ferrochrome, made in a second step: melt chromite with lime in an arc furnace and reduce it with ferrosilicon instead of carbon. Chromium metal and its chemicals are in Chromium and Its Compounds.
  • Ferronickel. Garnierite smelted with coke and iron in an arc furnace gives ferronickel with 20–40% nickel — fine for alloy steel. Pure nickel, for plating (Electroplating), needs much more chemistry (see Nickel and Cobalt).
  • Tungsten. Grind wolframite fine and melt it with about its own weight of soda ash. Boil the cooled mass in water: the tungsten dissolves as sodium tungstate, leaving iron and manganese behind. Add Hydrochloric Acid to the clear liquid: yellow tungstic oxide settles out. Wash it, dry it, mix it with 15–20% of its weight of charcoal powder, and heat it in a sealed crucible to about 1,400 °C for several hours to get grey tungsten powder. Or smelt the concentrate with iron and coke in an arc furnace to ferrotungsten. The full tungsten route, including lamp filaments, is in Tungsten and Filament Wire.
  • Vanadium and molybdenum are made in similar ways — in practice, as ferrovanadium and ferromolybdenum in the arc furnace (see Molybdenum).

Step by step: making an alloy steel

Either a crucible (Steel in Quantity) or an arc furnace will do. Robert Mushet made his tungsten tool steel in crucibles; Hadfield made his manganese steel the same way.

  1. Start clean. Use low-phosphorus, low-sulfur steel or scrap of known kind. Keep records of every charge.
  2. Calculate the additions.

    ferroalloy needed = (target % × bath weight) ÷ (% of the metal in the ferroalloy × recovery) Example: a 50 kg bath, aiming for 1.5% chromium, with ferrochrome of 60% chromium and a recovery of 0.9 (10% lost to the slag): 0.015 × 50 ÷ (0.6 × 0.9) = 1.4 kg of ferrochrome. Remember that high-carbon ferroalloys add carbon too.

  3. Melt and refine the base steel, remove the oxidising slag, and put on a reducing slag (lime with powdered charcoal) so the bath is quiet and oxygen-free. Chromium, manganese and vanadium burn away into an oxidising slag; nickel, tungsten and molybdenum do not.
  4. Add the alloys in order. Nickel and molybdenum can go in early with the charge. Tungsten is very dense: add it early and stir well so it does not lie on the bottom. Add chromium, manganese and vanadium last, warmed, in lumps the size of a walnut, 10–20 minutes before tapping.
  5. Stir, hold, sample. Stir with an iron bar, wait 10–15 minutes, take a spoon sample, and check it (below).
  6. Pour into dry, warmed moulds. Cool high-alloy ingots slowly — bury them in ash or dry sand — or they crack.

Working and heat treating

  • Alloy steels conduct heat poorly. Preheat slowly before forging or hardening, or the outside expands while the inside is cold and the piece cracks.
  • They are stiffer when hot. Forge at higher heats (bright orange to yellow) and stop at a full red; never hammer below dull red.
  • Anneal before filing or machining: heat to orange, then cool as slowly as possible in a box of ash. High-speed steel and Hadfield steel are still hard to cut: grind them instead (see Abrasives and Grinding Stones).
  • Follow the hardening heats in the table. High-speed steel needs a white heat, just short of melting, for a minute — far hotter than any carbon steel could survive — and two tempers, each of about an hour at 550–570 °C, which actually makes it harder.

How to tell it worked

  • The magnet. Austenitic stainless (18/8) and Hadfield manganese steel are not magnetic, or only faintly. Martensitic stainless and other alloy steels are magnetic.
  • The copper sulfate test. Clean a spot bright and put on a drop of copper sulfate solution (blue vitriol, see Electroplating). Ordinary steel turns copper-coloured within seconds; stainless steel stays clean.
  • The salt test. Leave a polished sample in damp salty air for a week. Stainless shows no rust; a light brown bloom means the chromium is too low or the carbon too high.
  • The spark test on the grindstone (see Steel): manganese steels give bright, bushy bursts; tungsten steels give short, dull red streaks with few bursts; stainless gives short, orange-tinged streaks with few forks; nickel steels give forked streaks.
  • Red-hardness. Heat a hardened high-speed steel tool and a carbon-steel tool together to a dull red, cool them, and try a file: the carbon steel is now soft; the high-speed steel is still hard.
  • Work-hardening. Hadfield steel dents under the first blows of a hammer, then becomes so hard that a file will not touch the hammered spot.

Note Troubleshooting. Chromium or manganese much lower than calculated → the slag was oxidising. Make a reducing slag first and add the alloys later. Stainless rusts → too much carbon (from high-carbon ferrochrome or electrodes) or too little chromium. Aim for at least 12% chromium and under 0.1% carbon; use low-carbon ferrochrome. Ingots crack while cooling → cooled too fast. Bury them in hot ash. Bars crack in the forge → forged too cold, or heated too fast. Soak longer at each heat. High-speed tool soft after hardening → not hot enough. It really must reach white heat. Protect the edge from burning by wrapping the tool in a little clay or packing it in charcoal. Hadfield steel brittle → quenched from too low a heat, or cooled slowly. Re-heat to 1,000–1,050 °C and quench in water.

Dangers

Danger Chromium compounds. The yellow chromates formed when chromium ore is melted with soda and saltpeter — and the fumes of stainless steel when it is welded or burned — cause cancer and severe skin ulcers. Never breathe the dust or fumes; wear gloves; never pour chromate solutions on the ground or into water others drink.

Danger Manganese fumes. Years of breathing manganese fume or dust — from furnaces, ferroalloy work, crushing ore or welding manganese steel — damages the brain and causes a shaking illness like Parkinson's disease. Crush ore wet, ventilate furnaces well, and rotate the work.

  • Nickel dust and salts cause skin allergies and, breathed over years, cancer. Wash after handling.
  • Acids and hot soda used to treat tungsten ore burn skin and eyes; see Acids, Bases and Testing.
  • Radioactive minerals. Bright yellow, powdery crusts with vanadium ores may be carnotite, which contains uranium. Do not crush, carry or store them near living spaces.
  • Molten metal and water, CO, and arc light — see Steel in Quantity and The Electric Arc Furnace.

What this unlocks

High-speed steel tools make Machine Tools fast enough for mass production and Precision and Interchangeable Parts. Alloy springs, bearings and gears are the core of the The Motor Vehicle, The Tractor, The Internal Combustion Engine engine and Gliders and Aeroplanes. Stainless steel serves kitchens, hospitals, breweries (Beer, Wine and Cider) and chemical works. Silicon steel makes efficient The Transformers and the Power Lines and Distribution possible. Nickel and chromium also give bright, rust-proof plating (Electroplating).

How it was first done

Around 1819–1822, Michael Faraday and the cutler James Stodart in London melted steel with nickel, silver, platinum and other metals in small crucibles, looking for better blades; their results were mixed but they were the first systematic alloy-steel experiments. In 1821 the French mining engineer Pierre Berthier noticed that iron–chromium alloys resisted acids. In 1868 Robert Mushet in England made a tungsten–manganese tool steel that hardened by cooling in air, and it was sold as "R. Mushet's Special Steel" for decades. In 1882 Robert Hadfield in Sheffield made his 12–14% manganese steel, and in 1900 he developed silicon steel for transformers. Frederick Taylor and Maunsel White in the United States showed high-speed steel at the Paris Exhibition of 1900: their tools cut steel so fast that they glowed red. Charles-Édouard Guillaume in Switzerland discovered invar in 1896. In 1912 Eduard Maurer and Benno Strauss at Krupp in Germany patented austenitic chromium–nickel stainless steel, and in 1913 Harry Brearley in Sheffield, looking for erosion-resistant gun barrels, found that a 12.8% chromium steel would not etch, and turned it into stainless cutlery.

Source: content/entries/metals/alloy-steels.md