Part 3 · Metals
Metal Spinning and Raising
How a flat disc of copper, brass, silver, pewter or aluminium becomes a seamless bowl, beaker, pan or lamp reflector — by hammering it into a hollow (sinking), crowding it up over a steel stake (raising) and smoothing it with a polished hammer (planishing), or, far faster, by pressing it onto a spinning wooden chuck on a lathe.
- Difficulty
- ●●●●●
- Time
- A day to sink a small bowl; two to four days to raise a beaker; minutes to spin a bowl once the lathe, chuck and tools are made
- Steps from zero
- 17 prerequisites →
This unlocks
—The full path from nothing — 17 steps before this one
- Stone Tools
- Cordage and Rope
- Fire
- Finding and Preparing Clay
- Finding and Identifying Ores
- Basic Woodworking
- Hunting and Trapping
- Charcoal
- Hides and Leather
- The Wheel and Axle
- Bellows
- The Lathe
- Gears
- Iron (the Bloomery)
- The Waterwheel
- Blacksmithing
- Sheet Metal and Rolling
- Metal Spinning and Raising
Do them roughly in this order. See it on the tech tree →
Why it matters
A seam can leak, rust, come unsoldered over a fire and trap dirt. A vessel made from one piece of metal cannot. For thousands of years coppersmiths and silversmiths made pots, cups and basins this way with a hammer, a stake and a fire to anneal — and you can too, once you have copper sheet (Sheet Metal and Rolling).
The lathe makes the same work fast: a spinner presses a disc onto a turning wooden form and has a bowl in five minutes. Spinning makes lamp founts and shades (Lamps and Candles), the parabolic reflectors of lighthouses, signal lamps, headlamps and torches (Harbours and Lighthouses, Dry Cells and Electric Torches), pans and kettles (Pots, Pans and Kettles), funnels, bells, bowls for laboratory work, horn bells for brass instruments (Horns, Pianos, Organs and Accordions) and the nose cones and ducts of machines.
Pressing in steel dies (Presses, Punches and Dies) wins for huge runs; for one piece to a few thousand, raising and spinning are far cheaper.
How it works
There are three ways to turn a flat disc into a hollow. All of them make the metal work harden — get stiffer and springier until it cracks — so you must anneal it (make it soft again with heat) between rounds of work.
- Sinking (hollowing). Hammer the disc into a hollow. The metal stretches: the middle thins while the outline stays nearly the same. Quick, but only for shallow bowls — no deeper than about a third of their width.
- Raising. Hold the disc tilted on a smooth stake (a steel anvil-head on a post) and strike just beyond where it touches. Each blow pushes metal down onto the stake and inward. The metal is crowded, not stretched, so the wall keeps the sheet's thickness. Slow, but it makes any depth, even necks narrower than the body.
- Spinning. Press a turning disc onto a wooden chuck of the inside shape with a smooth bar levered against a pin. Fast and even, but the piece must slide off the chuck — mouth wider than anything below it — unless the chuck comes apart.
Planishing finishes all three: light, overlapping blows of a polished hammer on a polished stake that fits the curve, smoothing the marks and work-hardening the vessel stiff.
| Metal | Anneal | Cool | Notes |
|---|---|---|---|
| Copper | Dull red, just visible in shade (about 600 °C) | Quench in water, or let cool | The easiest to raise. Anneal after every course. |
| Brass (70/30) | Dull red | Let it go black, then quench | Hardens quickly. Quenched from red it can crack. |
| Silver (sterling) | Dull red | Let the red go, then quench | Pickle off the dark scale after each anneal. |
| Aluminium | About 350–400 °C | Air | Gives no glow. Rub on a little soap: anneal until the soap mark turns black. |
| Pewter, lead | None needed | — | Too soft for much hammering; ideal for spinning (Tin and Pewter). |
| Mild steel | Bright red | Slowly in ash | Hard work. Raise hot if thick. |
Anneal whenever the metal rings instead of thudding and springs back instead of moving. Then pickle off the black scale in warm 1-in-10 Sulfuric Acid, hot alum water, or strong vinegar with salt, and rinse (Acids, Bases and Testing). Scale hammered in leaves pits that never polish out.
What you need
| Tool | Size | Make it from |
|---|---|---|
| Sinking block | A hardwood stump or end-grain log, 30–40 cm across, with shallow round hollows 5–15 cm across and 1–4 cm deep carved in the top | Beech, oak, elm |
| Sandbag | Leather bag 20–25 cm across, filled with fine dry sand | Hides and Leather |
| Doming hammer | Two ball-shaped faces, 25–40 mm across; 300–500 g | Tool steel |
| Raising hammer | Two long, narrow, rounded wedge faces, 35–50 mm long, 10–15 mm wide; 400–700 g | Tool steel |
| Planishing hammer | One flat face and one very slightly domed, 25–35 mm across, mirror-polished; 250–450 g | Tool steel |
| Mallets | Boxwood or hide, 50–60 mm across | Hardwood, rawhide |
| Raising stakes | Below | Steel, cast iron or hardwood |
| Dividers, compasses, calipers, a card template | Measurement from Scratch | |
| A forge, charcoal fire or blowlamp for annealing; pickle in a wooden or pottery tub | Charcoal | |
| For spinning: a rigid lathe with continuous rotation (treadle and flywheel, line shaft or motor), 500–1,500 turns a minute | Machine Tools | |
| Spinning chucks, follower, tools, tool rest | Below | Hardwood, steel |
| Lubricant | Tallow, beeswax, hard soap, lard | Butchery and Meat, Beekeeping, Soap |
| Polish | Pumice, tripoli, rouge | Abrasives and Grinding Stones |
Where to find it
Metals come from Copper Smelting, Zinc and Brass, Gold and Silver, Aluminium and Steel. From nature: close-grained hardwood for chucks and blocks (maple, beech, birch, apple, pear, boxwood, hornbeam; oak will do), tallow or beeswax for lubricant, sand and hide for the sandbag and mallets, and tripoli (a soft, pale, crumbly rock of fine silica) for polish.
Stakes and hammers
Raising stake
A stake is a smooth, hard steel head on a square tang (a shank) that drops into a square hole in a heavy post, a stump or an iron stake plate bolted to the bench. Every stake does one shape:
- T-stake — a long horizontal arm, 25–40 cm, one end thick and round (40–50 mm), the other narrower and flatter. Used for raising and for working the sides of tall shapes.
- Mushroom stake — a domed head 50–100 mm across. Planishing bowls and the bottoms of vessels.
- Side stake — an arm bent down at 30–45°, with a rounded edge. Raising from the base outward.
- Bottom stake — a flat round head with a sharp edge, for setting the corner where wall meets base.
- Horn — a long tapering cone, for the necks of jugs and for spouts.
Making a stake. Forge it from medium- or high-carbon Steel bar 30–40 mm square (Blacksmithing), with a tang 20–25 mm square and 15 cm long that fits its hole without rocking. Shape the head to a template, then smooth it with ever finer stones, emery and finally tripoli on leather to a mirror. Harden the face from cherry red and temper to straw (about 230 °C). Keep stakes greased and never hit one with a bare steel hammer — the bruise prints into every vessel planished there after.
A first stake can be a ground cast-iron head (The Blast Furnace and Cast Iron), a smooth boulder, or hardwood — beech or hornbeam carved to shape. Wood dents, but it is quick to make and fine for raising soft copper.
Hammers
Forge each from tool steel with a 30–35 cm ash or hickory handle (Hammers, Pliers, Wrenches and Screwdrivers). The raising hammer's narrow faces are curved along their length and rounded across, so they never cut a line into the metal. The planishing hammer's faces are mirror-polished and only very slightly domed. Harden and temper all faces to straw. A good hammer falls square of its own weight and bounces lightly off the work.
Method 1: Sinking a bowl
A first project. A copper disc 15 cm across and 1–1.2 mm thick makes a bowl about 12 cm across and 3–4 cm deep.
- Cut the disc with snips (Sheet Metal and Rolling) and file the edge smooth.
- Anneal and pickle.
- First course. Hold the disc tilted over the hollow and strike near the edge with the doming hammer, turning the disc a little after each blow — a ring of overlapping blows. Then a ring 1 cm further in, and so on to the centre. A sandbag works instead of a block.
- True the rim. When the edge waves, lay the bowl rim-down on a flat stake and tap the waves down with a mallet. Never let a wrinkle fold over.
- Anneal and repeat until deep enough: usually 3–5 courses.
- Planish (below) on a mushroom stake, and flatten a base: set the bowl on a flat stake and tap the bottom lightly from inside with a mallet so it stands without rocking.
- Finish the rim: file it level, then either thicken it by tapping the edge down on its own thickness all round (caulking), or wire it (Sheet Metal and Rolling).
Method 2: Raising a beaker or deep bowl
The coppersmith's saucepan is raised this way (Pots, Pans and Kettles). In detail, for a beaker 8 cm across and 10 cm tall:
- Size the disc. Base diameter plus twice the height: 8 + 20 = 28 cm, from 1–1.2 mm copper; this leaves a little to trim. Draw concentric circles 1 cm apart from the base circle outward to guide each course.
- Sink the base area slightly into a shallow hollow, so the disc becomes a dish. This gives you an edge to start raising from.
- Raise a course. With the stake at chest height, hold the dish tilted on it, touching at the base line. Strike just beyond the line of contact, driving the metal down onto the stake. Turn the work 1–2 cm per blow; after each round move out one circle, to the rim. The wall tilts up and shrinks in diameter.
- Anneal and pickle. Every course.
- Repeat. Each course raises the wall by about 5–15 mm. A beaker takes 8–12 courses; a tall vase twenty or more.
- Speed it up by crimping (fluting). After the first course, hammer the edge into a grooved hardwood block with a narrow wooden wedge, so the rim becomes a ring of evenly spaced folds like a pie crust, 2–3 cm deep. Then hammer the folds down flat onto the stake, starting at their roots. Each crimp gathers metal fast. Do not let folds fold over.
- Keep the rim thick. Every few courses, tap the rim down on its own edge so it stays as thick as the wall, or thicker. A thin, cracked rim is the commonest failure.
- Planish, set the base sharp on a bottom stake, trim the rim with a file and caulk or wire it.
Planishing
- Choose a stake that fits the curve closely — slightly more curved than the work, never less.
- Clean everything. Grit between hammer, work and stake leaves pits.
- Start at the centre of the base and work outward in a spiral, or in rings, with light blows that each overlap the last by half. Each blow should press the metal flat against the stake.
- Listen. A blow where the metal touches the stake makes a sharp, clean ring. A dull, hollow thud means a gap: move the work so the blow lands where it is supported.
- Two full passes, annealing between them if the work is copper, leave an even surface of small bright facets — a sign of good work, often left as the finish.
Method 3: Spinning on the lathe
The lathe
A pole lathe reverses every stroke and will not do (The Lathe). You need continuous rotation — a treadle with a heavy flywheel, a line shaft or an The Electric Motor (Machine Tools) — a rigid bed, a spindle in good Bearings and Lubrication, stepped pulleys for speed, and a tailstock with a revolving centre (a point turning in its own bearing, Making Ball and Roller Bearings).
| Disc diameter | Speed, turns a minute |
|---|---|
| 10 cm | 1,200–1,500 |
| 20 cm | 800–1,000 |
| 30 cm | 500–700 |
| 45 cm | 300–450 |
Slower for steel and thick metal; faster for soft aluminium and pewter.
Spinning chuck
The chuck is the inside shape of the finished piece, turned in wood.
- Glue up a block of dry, close-grained hardwood a little larger than the piece: for a bowl 20 cm across, a block 22 cm across and 10 cm thick. Glue layers with grain crossed, so it does not split (Glues and Adhesives).
- Screw it to an iron faceplate on the headstock spindle.
- Turn it with ordinary wood-turning tools (Wood Turning and Treen) to the exact inside profile, checking against a card or sheet-metal template. Leave the face that will form the bottom flat or very slightly hollow, and give every corner a radius of at least 3 times the sheet thickness.
- Sand smooth and rub in beeswax or tallow.
A hardwood chuck spins hundreds of pieces. For thousands, cast one in iron or turn it from steel (Metal Casting). For a shape narrower at the mouth (a vase), use a sectional chuck made of wedge-shaped segments around a central key; after spinning, pull the key and take the segments out one by one through the mouth.
Follower and tool rest
The follower is a leather-faced hardwood disc, a third to half the base diameter, on the tailstock centre; winding the tailstock in clamps the disc to the chuck. The tool rest is a stout iron bar beside the work with holes 2.5 cm apart for a smooth steel fulcrum pin 12–16 mm thick, moved hole by hole as the work goes on.
Spinning tools
Each is a steel bar 16–20 mm thick and 45–60 cm long, its end shaped, hardened, tempered to straw and polished like glass, in an ash handle 30–40 cm long that tucks under your arm for leverage.
| Tool | End shape | Use |
|---|---|---|
| Spoon (flat) | Broad, flat on one side, round on the other, rounded edges | The main tool: laying metal down in long sweeps, smoothing |
| Ball (round nose) | Hemisphere 12–20 mm | Starting the metal; tight corners |
| Point (trimming tool) | Sharp, square or pointed cutting tip, like a lathe tool | Trimming the edge true |
| Beading tool | A hardened grooved wheel on a fork, or a grooved tip | Rolling a bead or curling the rim over a wire |
| Backstick | A hardwood stick 3 cm square, 40–50 cm long, rounded end | Held on the far side of the flange to stop it wrinkling |
A roller tool — a hardened polished wheel 25–40 mm across turning on a pin in a forked bar — rolls instead of rubbing and lets you push harder with less heat. Make one when you can.
Spinning a bowl
- Cut the disc. For a shallow bowl, the blank diameter is about the length of the chuck's profile measured rim to rim with a tape laid over the curve, minus 5–10%, since spinning thins the metal a little. Start with soft aluminium 0.8–1 mm or annealed copper 0.6–0.8 mm.
- Mount it. Set the disc between chuck and follower, tighten lightly, and turn the lathe by hand. Tap the disc's edge with a stick until it runs true, then tighten hard.
- Lubricate the face of the disc with tallow, soap or beeswax.
- Set the base. Start the lathe. With the ball tool levered on the pin, press the metal against the chuck right beside the follower, so the bottom is locked in place.
- Sweep outward. With the spoon tool, press the metal toward the chuck in long, smooth strokes from the base outward toward the rim. Each stroke lays a little more metal on the chuck. Keep the unsupported part of the disc a cone, not flat and not too steep: lead it gradually, never trying to push the whole flange down at once.
- Fight wrinkles at once. If the outer flange starts to buckle into waves, hold the backstick behind it, opposite the tool, and squeeze the waves flat between them. Wrinkles that are left grow and fold.
- Trim. When the edge goes ragged or uneven, trim a few millimetres off with the point tool.
- Anneal copper and brass when they squeak, harden and resist the tool: take the work off, anneal, pickle, remount. Aluminium of this thickness rarely needs it for a bowl.
- Finish. Smooth the whole surface with the flat side of the spoon tool. Trim the edge to final size, then roll it over into a bead or curl it round a wire with the beading tool for strength and safety.
- Polish on the lathe with pumice, then tripoli, then rouge on a pad of cloth. Take it off.
A practised spinner makes a small bowl in five minutes.
Spun objects
Spun bowl
A good bowl runs true when spun on a finger, has walls even within 0.1–0.2 mm (check with calipers at four points), no wrinkles or tool chatter, and a rolled or beaded rim. Typical: 15–25 cm across, 0.8 mm aluminium or copper. Copper bowls for food or acid must be tinned inside (Tin and Pewter).
Parabolic reflector
The rule for the curve and how to place the flame are in Harbours and Lighthouses and Dry Cells and Electric Torches. To make one:
- Cut a template of the parabola from thin sheet metal, accurate to 0.2 mm, by plotting points on squared paper (Geometry and Trigonometry).
- Turn a hardwood or, better, cast-iron chuck to the template. Any error in the chuck becomes a smeared beam.
- Spin a disc of 0.6–0.8 mm copper, brass or aluminium onto it. Spin the rim into a stiff flat flange or bead; reflectors lose shape if they flex.
- Leave a hole at the vertex (the bottom) for the lamp or bulb holder, and trim it on the lathe.
- Polish the inside to a mirror: pumice, tripoli, rouge. Then silver-plate copper or brass (Electroplating, Mirrors) and lacquer it, or keep aluminium bright with a coat of clear lacquer.
- Test: set a candle or bulb at the focus in a dark room and look at the beam on a wall 5–10 m away. A good reflector throws an even round patch with sharp edges. Slide the light along the axis until the patch is smallest.
Lamp parts and pans
Oil-lamp founts (two spun halves soldered together), burner galleries and conical shades are spun (Lamps and Candles, Lanterns, Gas Lamps and Lighters). Pans (Pots, Pans and Kettles) are spun from 1–1.5 mm aluminium or copper over a flat-faced chuck with a well-rounded corner, the rim stiffened with a bead.
How to tell it worked
- Thickness. Calipers at the rim, mid-wall and base. Raised work: about the original sheet thickness everywhere. Sunk work: thinnest in the middle of the base. Spun work: within 10–20% of the original.
- No cracks. Look closely at the rim after every anneal. A hairline crack at the edge will run across the piece; file it out at once, in a smooth curve, and keep going.
- Sound. A planished vessel rings clearly when flicked. A dull or buzzing note means a crack.
- Shape. Check against the template. Spun pieces should run true on the chuck with no wobble at the rim.
Note Troubleshooting. Metal folds over into a pleat → you went too fast or let a wrinkle grow. Hammer or spin it out at once while small; once folded, it is a crack. Rim splits → work-hardened rim, or the rim was let go thin. Anneal more often and caulk the rim. Pits and dents that won't polish out → scale or grit hammered in, or a marked hammer or stake face. Pickle every time; polish your tools. Spun metal tears near the base → pushed too steeply or too fast; ease the angle, more lubricant, anneal. Spun piece won't come off the chuck → the chuck has an undercut, or swelled with damp. Give chucks a slight draft and keep them dry. Tool chatters and leaves ridges → tool rest loose, pin too far from the work, or a rough tool. Move the pin close, polish the tool.
Dangers
Danger The spinning lathe can throw the work and the tool. If the follower slips, a sharp-edged disc flies off the lathe like a blade. Tighten the tailstock hard, check it every few minutes, and never stand in line with the disc's plane when starting. If a tool catches, the long handle can whip up into your face or ribs: keep the fulcrum pin close to the work and the tool pressed firmly to the pin. Tie back hair, wear no loose sleeves, take off rings, and never reach over the turning work.
- Hearing. Raising and planishing on steel stakes is very loud, hour after hour. Coppersmiths went deaf. Plug your ears with wax and wool.
- Sharp edges. Spun and cut edges slice like knives. File them and wear leather gloves when handling raw discs — but never gloves at the lathe, which can catch.
- Hot metal and acid. Annealed work looks cold long before it is. Pickle burns skin and eyes; add acid to water, not water to acid (Acids, Bases and Testing).
- Copper and brass dust from polishing irritates the lungs. Polish wet or in moving air.
What this unlocks
Seamless hollowware — bowls, beakers, jugs, pans and kettles (Pots, Pans and Kettles, Cutlery and Tableware); reflectors for lamps and lighthouses (Harbours and Lighthouses, Signal Fires, Flags, Semaphore and Heliographs); parts of Lanterns, Gas Lamps and Lighters, horn bells, laboratory basins (Burners, Stands and Laboratory Equipment) and machine covers. The same chucks guide deep drawing in Presses, Punches and Dies when the run is long enough to pay for steel dies.
How it was first done
Hammered metal vessels are as old as metal. Cups and bowls of hammered copper, silver and gold were made in Mesopotamia and Egypt in the third millennium BC; the royal graves at Ur (about 2600–2400 BC) held raised gold and silver vessels of great skill. Raising, sinking and planishing were the core of the silversmith's and coppersmith's trades from then on, and the tools — stakes, hammers and an annealing hearth — hardly changed for four thousand years.
Spinning on the lathe is younger and its origins are poorly recorded; some claim very ancient roots, but there is little firm evidence. By the early 1800s, English workshops in Sheffield and Birmingham were spinning Britannia metal (a hard pewter of tin, antimony and copper) into teapots and jugs, and the trade spread to America around the 1840s. Spinning grew with aluminium in the 20th century, for cookware, lamp reflectors, aircraft parts and the nose cones of rockets.
Source: content/entries/metals/metal-spinning-and-raising.md