◆ Rebuild

Part 8 · Chemistry

Dyes and Mordants

Colour wool, silk, linen and cotton with plants — red from madder roots, yellow from weld, brown from walnut hulls, and blue from woad or indigo leaves in a fermenting vat. Mordants such as alum, iron and tannin lock the colour into the fibre so it survives sun and washing.

Difficulty
●●●●●
Time
A day for a mordant-and-dye batch of wool; one to two weeks to start a fermentation indigo vat; three years to grow madder roots
Steps from zero
3 prerequisites →

You need first

Pottery

This unlocks

Colour Photography
The full path from nothing — 3 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Pottery
  4. Dyes and Mordants

Do them roughly in this order. See it on the tech tree →

Why it matters

Undyed wool is cream, grey or brown; linen is grey-beige. Colour marks family, trade and office, makes a warning flag visible a kilometre away, and lets a weaver pattern cloth by dyeing the threads first. For thousands of years dyed cloth was among the most valuable things traded anywhere.

Dyeing is also your first real chemical industry: controlled temperatures, measured salts, acids and alkalis, and reactions inside a pot you cannot see into. The same skills lead to Pigments, Paints and Varnish, Ink and Acids, Bases and Testing, and alum is also used for Hides and Leather and Paper.

This chapter covers four great dye plants — woad (or tropical indigo) for blue, madder for red, weld for yellow and walnut for brown — and the mordants that make them last. By dyeing one colour over another, they give almost every colour people wore before 1856.

How it works

A dye is a coloured substance that dissolves in water and then attaches itself to fibre. (A pigment, by contrast, does not dissolve; it is ground fine and glued onto a surface — see Pigments, Paints and Varnish.) There are three ways a dye can hold on:

  1. Substantive dyes cling to fibre on their own. Walnut hulls, tea, onion skins and most barks are like this. They are easy, but they give mostly browns, tans and dull yellows.
  2. Mordant dyes need a go-between. A mordant (from French mordre, "to bite") is a metal salt — usually alum (an aluminium salt), iron or copper — that is first soaked into the fibre. The metal grips the fibre with one hand and the dye with the other, and the combined "lake" is insoluble, so it will not wash out. Madder and weld are mordant dyes. The mordant also changes the colour: madder on alum is red, on iron it is purple-brown to black.
  3. Vat dyes do not dissolve in water at all — indigo is the famous one. In a vat, an alkaline liquid with a chemical that removes oxygen turns blue indigo into a soluble yellow-green form. Cloth dipped in it soaks it up; lifted into the air, the dye takes back oxygen and turns blue again, now trapped inside the fibre.
With a mordant: the dye is locked on Without a mordant: the dye rinses away Same dye, different mordant Dyemadder Mordantaluminium Fibrewool Wash watercarries thecolour off Alum Iron Madderroot Weldyellow plant Walnutno mordantneeded Indigoa vat dye red purple-brown bright yellow olive green brown; iron makes it near black blue on any fibre
Fig. 1 How a mordant works. Alum soaked into the fibre gives aluminium that binds to the fibre on one side and the dye on the other, so the colour cannot wash out. The same dye on a different mordant gives a different colour.

Fibre matters. Animal fibres — Wool and Silk — are made of protein, which grabs dyes and mordants eagerly. Plant fibres — linen and Cotton — are cellulose, which grabs very little. They need an extra first step: soaking in tannin (from oak galls or bark), which sticks to cellulose and then holds the alum. Expect linen and cotton to come out paler than wool from the same bath; deep colours on them take repeated rounds.

Heat matters. Most mordant dyes release their colour at 60–80 °C. Boiling often dulls them: madder turns from red to brick-brown above about 80 °C. Wool also felts and shrinks if heated or cooled suddenly, or stirred hard while hot (see Felt). Raise and lower temperature slowly.

What you need

Quantities in dyeing are given as a percentage of the dry weight of the fibre ("WOF"). For 1 kg of dry wool, "10% alum" means 100 g of alum.

Item Amount per 1 kg of dry fibre Notes
Dye pot 30–40 litres Glazed stoneware (Glazes), copper, brass or iron. Iron and copper pots shift colours (see below). Never use it for food again.
Water 30–40 litres Rain water is best. Very hard or iron-rich water dulls colours.
Alum 100–120 g (wool), 150–200 g (linen, cotton) See "Making alum" below
Cream of tartar (optional) 60–70 g The crust inside wine casks (Beer, Wine and Cider); makes wool softer and colours brighter
Tannin 80–100 g of ground oak galls, or 300–500 g of oak or sumac bark For linen and cotton
Green vitriol (iron) 10–30 g To darken colours. See Sulfuric Acid
Madder root, dried and ground 0.5–1 kg Red
Weld, dried whole plant 0.5–1 kg Yellow
Walnut hulls, green or blackened 1–2 kg Brown, no mordant needed
Indigo pigment 20–50 g for a small vat Blue; extracted from woad or indigo leaves
Stale urine, wood ash lye, slaked lime, very ripe fruit See the vat recipes For indigo vats (Lye and Potash, Lime)
Stirring sticks, wooden tongs, a long pole, cloth for straining Smooth, so they do not snag fibre

Dye wool as loose fleece or skeins of yarn tied loosely in 2–3 places with a figure-of-eight tie. Cloth can be dyed whole but takes colour less evenly.

Where to find it

Full descriptions of each plant are in the materials glossary.

  • Woad — blue-green rosettes of spoon-shaped leaves on dry, chalky or disturbed ground in Europe and western Asia; yellow flowers in its second year. Sow in spring; cut the leaves every 4–6 weeks from mid-summer.
  • Indigo plants — true indigo (Indigofera), a pea-family shrub of the tropics, and Japanese indigo (Persicaria tinctoria), a knotweed grown as an annual in East Asia. Both give several times more dye than woad. All indigo-bearing leaves turn blue-black where bruised — a quick field test.
  • Madder — a clinging, prickly, square-stemmed plant with whorls of narrow leaves; its roots are red inside. Wild madder and bedstraw roots (Galium) give weaker reds and pinks. It needs three years to make good roots: plant a bed now.
  • Weld — a thin spike of tiny greenish-yellow flowers up to 1.5 m tall, on chalky waste ground; harvest the whole plant in flower. Other yellows: dyer's broom, goldenrod, tansy, chamomile, birch leaves, onion skins (less fast).
  • Walnut — the green outer husks, gathered as they fall in autumn; they blacken and stain fingers within minutes. Alder bark and cones and oak bark give similar browns.
  • Tannin — oak galls (Ink), and the bark of oak, chestnut, sumac leaves and pomegranate rind (see Hides and Leather). Chew a sliver: strong puckering means strong tannin.
  • Iron — green vitriol from weathered pyrite (Sulfuric Acid), or an iron liquor made by soaking rusty iron scrap in vinegar (2 parts vinegar to 1 part water) for two weeks.
  • Alum — see below. Some clubmosses (Diphasiastrum, Lycopodium), low creeping evergreen plants of northern forests and moors, store so much aluminium that in Scandinavia their dried stems were boiled with wool as a mordant: about equal weight of dried clubmoss to wool.

Making alum

Alum is potassium (or ammonium) aluminium sulfate: colourless crystals with a sweetish, intensely puckering taste. It is the most important mordant ever used — bright, clean colours, and far less poisonous than copper or tin salts. It is made from alum shale (dark shale speckled with pyrite, whose weathered surfaces grow astringent white crusts) or from alunite (a whitish rock of volcanic districts). The short recipe below is enough for dyeing; Alum and Alumina gives the full treatment, including alum from ordinary clay and sulfuric acid.

From alum shale (the English method, 1600s–1871):

  1. Stack the broken shale in a long heap over brushwood and burn it slowly for weeks to months, as for Charcoal. The pyrite burns and turns the clay in the shale into aluminium sulfate. The heap turns red.
  2. Leach the burnt shale with water in clay-lined pits, as you would leach ashes for Lye and Potash. Run the liquor through several pits until a fresh egg just floats in it.
  3. Boil it down by about half in a lead or stoneware pan.
  4. Add potash or stale urine. Aluminium sulfate alone will not crystallise well; it needs potassium or ammonium. Stir in potash (Lye and Potash) or old urine (rich in ammonia) — roughly one part potash to ten parts of the boiled liquor, or about a third of the volume in urine — until a test drop on a cold stone grows crystals.
  5. Run it into wooden or clay tanks and leave it 4–6 days. Alum grows on the walls as clear crystals. Rinse them in cold water, redissolve in the least boiling water, and crystallise again for a purer product.

From alunite: roast the stone at a dull red heat for a few hours, heap it in the open and keep it wet for several weeks until it crumbles, then leach and crystallise as above.

Tip Is it alum? Clear, eight-sided crystals; taste a crumb — sweet then fiercely drying, not salty, not bitter-metallic. A pinch heated on a sherd froths up into a white, puffy, light mass. Green vitriol, by contrast, is pale green and tastes inky.

Preparing the fibre

  1. Scour first. Grease and dirt make blotchy colours. Wash fleece or yarn in warm (50 °C, hand-hot) soapy water (Soap) or soapwort, or soak overnight in one part stale urine to three parts warm water. Rinse at the same temperature. Boil linen and cotton for an hour in water with a cupful of wood-ash lye.
  2. Wet it out: soak the fibre in plain water for at least an hour before any bath. Dry fibre takes colour unevenly.

Method 1: Mordanting with alum

Wool and silk:

  1. Dissolve 10–12% alum (and 6–7% cream of tartar if you have it) in a little boiling water, then stir it into the dye pot filled with 30–40 litres of lukewarm water per kilogram of wool.
  2. Add the wet wool. Heat slowly — over about an hour — to 80–90 °C: too hot to keep a finger in for more than a second, steaming strongly but not bubbling. Silk: no hotter than 70 °C.
  3. Hold it there one hour, turning the wool gently every 15 minutes.
  4. Let it cool in the bath, overnight if you can. Lift out, squeeze gently, and either dye at once or dry and store it.

Linen and cotton: first soak overnight in a warm bath of tannin (80–100 g ground oak galls per kg, simmered for an hour and strained). Wring out, then put into a hot bath with 15–20% alum and leave overnight. Rinse lightly. For deep colours, repeat the tannin-and-alum steps two or three times.

Iron is used differently: it is added after dyeing, in a separate short bath. See "Changing the colour" below.

Method 2: Madder, weld and walnut

Madder (red)

  1. Use roots from plants at least three years old, dug in autumn, washed, dried and ground or chopped fine. Use 50–100% of the wool's weight: 50% gives orange-red, 100% deep red.
  2. Soak the ground root overnight in a little warm water. Many dyers pour off and discard this first yellowish water — it holds brown and yellow colours that dull the red.
  3. Put the root (in a cloth bag if you want to avoid picking bits out of the wool) in the dye pot with 30–40 litres of water and a teaspoon of crushed chalk per kilogram of wool. Madder reds need calcium; in soft rain water they come out brownish.
  4. Add the alum-mordanted, wet wool. Heat slowly over an hour to 60–70 °C — hot to the hand, steaming, but never near boiling. Above about 80 °C the red goes brown.
  5. Hold 1–2 hours, turning gently. Cool in the bath.
  6. Rinse until the water runs clear, then wash in warm soapy water.

The same roots can be used two or three times for paler reds, pinks and oranges ("exhaust baths").

Weld (yellow)

Chop the dried plant, simmer it in water for one hour at 80–90 °C, strain, and add the alum-mordanted wool. Hold at 70–80 °C for an hour. Use 50–100% WOF. A pinch of chalk or a splash of lye makes the yellow brighter and more golden. Weld is the most light-fast yellow of the temperate plants.

Walnut (brown)

Fill a pot with green or blackened walnut hulls (100–200% of the fibre's weight), cover with water, and let them soak for a week or more — the liquor turns black-brown. Then simmer the hulls for an hour, strain, add wet, unmordanted fibre and hold at 80–90 °C for 1–2 hours. Walnut needs no mordant. It is the easiest dye in this book and very fast.

Method 3: Indigo from woad and the indigo vat

Indigo gives the only really fast blue from plants, and it works on wool, silk, linen and cotton equally well. It is a two-stage job: first get the blue pigment out of the leaves, then dissolve it in a vat.

1. Blue indigo 2. The vat 3. Lift into the air does not dissolve in water + alkali stale urine, lime water or ash lye + oxygen-taker bacteria (urine vat) or fruit sugar (fruit vat) Coppery skinand blue froth Clear yellow-greendissolved indigo Kept warm35–40 °C urine vatabout 50 °C fruit vat greenturningblue 0 s30 s1 min Oxygen from the airturns it blue again, nowlocked inside the fibre Dip again5–10 dips for navy
Fig. 2 The indigo cycle. Blue indigo is insoluble. In the vat, bacteria or fruit sugar and an alkali take oxygen from it and turn it into a soluble yellow-green form. Cloth soaks this up; lifted into the air, it turns green and then blue within a minute.

Extracting indigo pigment from fresh leaves

  1. Cut 5–10 kg of fresh leaves on a dry morning and use them within hours.
  2. Chop them into a pot, cover with water at about 80 °C (just too hot to keep your hand in) and weigh them down for 10–15 minutes for woad — or soak tropical indigo leaves in cool water for 12–24 hours until the water turns yellow-green with a coppery film.
  3. Strain and squeeze out the leaves, and cool the liquid fast in a tub of cold water.
  4. Make it alkaline: stir in lime water (clear water from settled slaked lime, Lime) or wood-ash lye a cupful at a time until the liquid turns a darker green and feels slightly slippery between finger and thumb — about 1 litre of lime water per 10 litres of liquid.
  5. Beat in air for 10–20 minutes: whisk it with a bundle of twigs, or pour it repeatedly from one pot to another from shoulder height. The froth goes from yellow to green to blue. Stop when fresh froth stays blue and soon collapses.
  6. Leave it to settle overnight. Blue sludge sinks to the bottom. Carefully pour off the clear yellow-brown water above it.
  7. Pour the sludge into a cloth bag, let it drain, then dry it in the shade into a blue-black cake. Grind to powder.

Expect roughly 1–3 g of indigo per kilogram of fresh woad leaves — woad is poor — and several times more from tropical indigo. A small vat needs 20–50 g, so grow plenty.

The urine vat (the oldest)

  1. Collect 10 litres of urine and leave it in a covered pot for 2–4 weeks until it smells strongly of ammonia. (Stale urine is alkaline and full of the right bacteria.)
  2. Grind 20–30 g of indigo with a little of the urine in a mortar into a smooth ink, and stir it into the pot.
  3. Keep it warm, 35–40 °C — blood heat — for one to two weeks: stand the pot in a box of fermenting horse dung, or bury it in warm ash beside the fire, or keep it in a sunny, sheltered spot wrapped in straw. Stir gently once a day.
  4. The vat is ready when the liquid under the surface is clear yellow-green, with a coppery, shiny film on top and a crust of blue bubbles (the flower). A drop on a white sherd should turn from yellow to blue in about a minute.

The lime-and-fruit vat (fast)

This works within hours and needs no warmth for days:

  1. Grind 10 g of indigo to a paste with a little water.
  2. In a 10-litre pot of water at about 50 °C, stir in the indigo, then 20 g of slaked lime and 30 g of fruit sugar — about 150–300 g of very ripe, mashed fruit (bananas, dates, pears, figs, grapes) or the same weight of honey. (The proportion 1 : 2 : 3 by weight of indigo, lime and sugar is easy to remember.)
  3. Stir gently, cover, and keep warm. In 1–3 hours it should turn yellow-green with a coppery skin. If it stays blue, add a little more fruit; if it is muddy and smells sour, add a little more lime.

Dipping

  1. Skim off the flower and set it aside on a plate. Wet the fibre and squeeze it out.
  2. Lower it in slowly, without splashing or dragging bubbles in — air spoils the vat. Hold it below the surface for 1–5 minutes, working it gently.
  3. Squeeze it out under the surface, then lift it out. It comes out yellow-green and turns blue in the air within a minute. Open it out so the air reaches everywhere.
  4. Let it oxidise 10–20 minutes, then dip again. Each dip deepens the colour: 1–2 dips give pale blue, 5–10 navy. Many short dips give a deeper, faster colour than one long one.
  5. Finally rinse, soak for 10 minutes in water with a splash of vinegar to neutralise the alkali, and wash with soap.

Return the flower to the vat and cover it. A well-kept vat lasts months; feed it more urine or fruit, and a little lime or ash when needed.

Note Troubleshooting the vat. Liquid is blue, not yellow-green → the indigo is not reduced. Too cold, too little fruit or not enough fermentation. Warm it and wait; add fruit or fresh stale urine. Colour rubs off the dyed cloth → loose indigo on the surface; dips too long or vat too strong. Many short dips, then wash well. Vat smells putrid and does not work → not alkaline enough. Add lime water or lye, a cup at a time. Blotchy colour → the fibre was greasy, or went in dry, or air bubbles were trapped. Scour and wet out properly.

Changing the colour

  • Iron "saddens". After dyeing, dissolve 1–3% green vitriol in a separate bath of warm water, add the wet fibre for 5–15 minutes, then rinse well. Yellows become olive and green, reds become purple-brown, browns become near black. Tannin-dyed cloth (oak galls, bark) plus iron gives grey to black — the same reaction as Ink. Too much iron makes wool harsh and brittle and slowly rots it; do not exceed 3%.
  • Alkali (a splash of lye or lime water in the rinse) shifts madder towards crimson and weld towards gold. Acid (vinegar) shifts them towards orange and lemon.
  • Overdyeing. Dye in indigo first, then in weld, for green (the famous "Lincoln green" was woad over weld). Indigo then madder gives purple. Madder then weld gives orange. Weld then walnut gives gold-brown.

How to tell it worked

Test a small sample before trusting a whole batch:

  • Wash test. Tie a tuft of white, undyed wool to your dyed sample and wash both in hot soapy water, rubbing hard. Good dye barely tints the white tuft and the sample looks the same afterwards.
  • Rub test. Rub the dry sample firmly ten times against a white cloth. Indigo that rubs off blue was dipped too long or not washed enough.
  • Light test. Cut a sample in two. Keep one half in the dark, in a book. Pin the other half in a sunny window for 3–4 weeks, half covered with card. Compare. Madder, weld, indigo and walnut on proper mordants barely fade. Onion skin, berries and most flower petals fade badly; they are "fugitive".
  • Even colour. Looking along a skein, there should be no pale tie marks or dark blotches.

Note Troubleshooting. Colour washes out → no mordant, too little mordant, or the bath was too cool or too short. Mordant again and redye. Madder came out brick-brown → overheated, or soft water. Keep below 70 °C and add chalk. Wool shrank and went stiff → felted by sudden temperature changes or rough stirring. Heat and cool slowly; let baths cool before moving wool between them. Patchy colour → greasy fibre or crowded pot. Scour well and use at least 30 litres of water per kilogram. Colours dull and muddy → iron in the water or pot; a dirty dye bath; overheating. Use rain water and a glazed pot.

Dangers

Warning Copper and tin mordants and arsenic or chrome mordants are poisonous. Some old recipes use blue vitriol (copper), tin salts, chrome or even arsenic. Avoid them all; alum and iron do nearly everything. Never use a dye pot, stirring stick or mordant spoon for food. Store mordants in labelled, lidded pots out of reach of children — a mouthful of green vitriol or blue vitriol can kill a small child.

  • Scalds. A full 40-litre pot is heavy; set it on a stable hearth and lift fibre with sticks.
  • Lime and lye burn eyes and skin; cover your eyes when mixing vats, and rinse any splash for 15–20 minutes (Lime, Lye and Potash).
  • Dust from madder, galls and mordants irritates the lungs. Grind damp.
  • Burning alum shale gives off choking, lung-damaging sulfur dioxide for as long as the heap smoulders. Site the heap well away from houses and work upwind of it.
  • Urine vats: keep covered, use urine from healthy people, wash hands with soap after.
  • Waste. Pour spent mordant baths onto waste ground far from wells and streams; iron baths kill fish.

What this unlocks

Dyed yarn makes patterned cloth, coloured Sewing, Needles and Thread thread, Felt and Knitting, Crochet and Netting. Madder precipitated onto alum gives the crimson pigment "rose madder" (Pigments, Paints and Varnish). Alum also tans white Hides and Leather, sizes Paper and settles mud out of drinking water. The search for dyes led to synthetic dyes from coal tar (Coal Tar Chemicals), which founded the modern chemical industry and the first synthetic medicines (Sulfa Drugs).

How it was first done

The oldest known indigo-dyed cloth is cotton from Huaca Prieta in Peru, about 6,000 years old. Madder-dyed cotton has been found at Mohenjo-daro in the Indus Valley (around 2500 BC), and Julius Caesar wrote that the Britons coloured themselves blue with vitrum, probably woad. Alum was traded across the ancient Mediterranean; when supplies from Turkey were cut off, the discovery of alunite at Tolfa near Rome in the 1460s made a fortune for the Papacy, and in the early 1600s England began making alum from Yorkshire shale, using shiploads of urine from London. Tropical indigo, imported by sea from India from the 1500s, slowly ruined the European woad growers. In 1856 an 18-year-old London student, William Henry Perkin, made the first synthetic dye, mauveine, from coal tar. Synthetic alizarin (the red of madder) followed in 1868 and synthetic indigo went on sale in 1897; within a generation the great dye fields of Europe and India were gone.

Source: content/entries/chemistry/dyes-and-mordants.md