◆ Rebuild

Part 3 · Metals

Metal Casting

Pour liquid metal into a hollow shaped like the thing you want, and let it set. This chapter covers patterns, sand moulds in boxes, clay and stone moulds, cores, sprues and risers, pouring, shrinkage and the faults that spoil castings — and lost-wax casting in depth.

Difficulty
●●●●●
Time
An afternoon for an open mould; a day to make a pattern and ram a sand mould; a week for a large lost-wax casting
Steps from zero
12 prerequisites →

You need first

Copper SmeltingFinding and Preparing Clay

This unlocks

Jewellery, Beads and Medals
The full path from nothing — 12 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Bellows
  12. Copper Smelting
  13. Metal Casting

Do them roughly in this order. See it on the tech tree →

Why it matters

Hammering can make a blade or a sheet. It cannot make a bell, a pot with legs, a gear wheel, a pump body or a thousand identical buttons. Casting can: make a hollow in the shape you want, fill it with liquid metal, and when it sets you have a part no smith could forge.

Casting is how you will make Gears, Bearings and Lubrication, the cylinders and valves of pumps and the The Steam Engine, the parts of a The Lathe and of Machine Tools, bells, type for Printing, and the pots and pans of the kitchen. You have already met simple casting in Copper Smelting and Bronze. This chapter turns it into a craft that can make almost any shape, again and again, from any metal you can melt: tin and pewter, Lead, zinc and brass, gold and silver and, later, The Blast Furnace and Cast Iron.

How it works

  1. The mould is the negative. It is a hollow (the cavity) exactly the shape of the part, inside a material that can stand the heat: stone, fired clay, or sand held together with a little clay.
  2. Metal must get in, and air must get out. Metal enters through a funnel called the pouring basin and a vertical channel called the sprue, then flows sideways along a runner and through a narrow gate into the cavity. Air and steam escape through vents — thin holes from the cavity to the outside — and up the riser.
  3. Metal shrinks as it sets. Liquid metal takes up more room than solid metal. As a casting freezes, the outside sets first and the last liquid, in the thickest part, shrinks away and leaves a hole called a shrinkage cavity. The cure is a riser: a reservoir of extra metal above the thickest part that stays liquid longest and feeds metal down into the casting as it shrinks. The riser is cut off afterwards.
  4. The solid shrinks too. After setting, the casting keeps shrinking as it cools to air temperature. So every pattern (the model you use to make the cavity) must be made a little larger than the finished part:
Metal Melts at Pour at (about) Glow colour at pouring Make the pattern larger by
Tin, pewter 232 °C (tin) 280–330 °C No glow; a slip of paper browns 0.5–1% (5–10 mm per metre)
Lead 327 °C 380–450 °C No glow 1%
Zinc 420 °C 450–500 °C No glow; dry pine shaving chars 1–1.5%
Brass 900–940 °C 1,000–1,050 °C Orange-yellow 1.5%
Bronze (10% tin) about 1,000 °C 1,100–1,150 °C Orange-yellow to yellow 1.5%
Copper 1,085 °C 1,150–1,200 °C Yellow 2%
Cast iron about 1,150–1,200 °C 1,300–1,400 °C Yellow-white 1%
  1. Water is the enemy. Any water in a mould turns to steam the instant hot metal touches it. A little steam makes bubbles in the casting; a lot throws molten metal out of the mould. Clay and stone moulds must be bone-dry and preheated. Sand moulds contain a little water on purpose (it is what makes the clay sticky), so they must be well vented and never wetter than needed.

Choosing a kind of mould

Open and two-piece moulds of stone or fired clay (see Copper Smelting and Bronze) are reusable and best for flat or simple shapes: ingots, axes, sinkers, buttons. Green-sand moulds in a wooden box make gears, wheels, brackets and machine parts, as many copies of one pattern as you like. Loam moulds make bells and big round vessels. Lost-wax moulds make anything at all — figures, hollow parts, undercuts, fine detail — but each mould gives only one casting. This chapter covers sand and lost wax in full, and the rules that apply to all of them.

What you need

Item Amount Notes
Moulding sand 50–100 kg for a small foundry Fine sand with 8–12% clay; see below. It is reused for years.
Parting dust A pouch Very fine, dry, non-sticky powder: charcoal dust, wood ash, crushed fired brick, or dry fine sand
Flask One, about 30 × 25 cm, two halves 8–10 cm deep A wooden frame in two halves; see below
Patterns One per shape Close-grained wood (pear, cherry, maple, pine), wax, clay, or an old casting
Rammer 1 A hardwood stick 40 cm long, one end wedge-shaped, the other end flat and 5 cm across
Riddle 1 A sieve with 3–4 mm holes: a basket, a perforated pot, or a cloth stretched on a frame
Small tools 3 mm vent wire, two tapered wooden pins (2–3 cm thick), a trowel or bone spatula, a feather
Crucible, furnace, tongs See Copper Smelting; for big crucibles, a forged iron ring with two long handles (a shank)
Beeswax, pine resin, clay, grog 0.2–2 kg wax For lost-wax moulds. See Beekeeping, Finding and Preparing Clay

Where to find it

Moulding sand. The best sand is fine (grains like table salt or finer), sharp-grained, and naturally mixed with a little clay — enough to hold a shape, not so much that it will not let steam through. Look in old river terraces, the banks of slow streams, and the edges of clay pits where sand and clay layers meet. Many foundries in history became famous for a local "loamy" sand.

Test a handful. Dampen it until it feels just cool and moist, like a garden after light rain — not shiny wet. Squeeze it hard in your fist.

  • Good: it keeps the exact print of your finger creases, and when you break the lump in two it snaps with clean, sharp edges and does not crumble or smear your palm.
  • Too little clay: it crumbles as you open your hand. Mix in fine clay.
  • Too much clay: it feels sticky, smears, and is hard to break. Mix in clean sand. It will also choke the steam and give blowholes.

Making it yourself. Sieve fine river sand, and dry and powder some good Finding and Preparing Clay. Mix 10 parts sand to 1 part clay by weight, dry, then knead in water a little at a time until the squeeze test passes — usually 4–6 parts water per 100. Leave it covered overnight so the water spreads evenly. For iron, founders mixed in 2–5% of fine charcoal or coal dust for a smoother surface.

Stone for permanent moulds. Soapstone (very soft, greasy-feeling grey-green stone that you can carve with a knife or a sharp flint) is the finest; it takes detail and does not crack in heat. Fine-grained sandstone works for simpler shapes. Avoid flint, quartz-rich granite and anything with water trapped in it: they shatter when heated.

Cuttlefish bone — the white, chalky, oval "bone" that washes up on many beaches — is soft enough to press a small model into.

Patterns

A pattern is a copy of the part you want to cast, used to press its shape into sand. It is usually carved in wood. A good pattern is the most valuable thing in a foundry: it makes thousands of castings.

  • Draft. Every face that lifts out of the sand must slope slightly so the pattern pulls out cleanly: 1–2 mm for every 10 cm of depth. Overhangs that would trap the pattern (undercuts) are impossible in a two-part sand mould; split the pattern, use a core, or use lost wax.
  • Allowances. Make every dimension larger by the shrinkage in the table above, plus 2–3 mm wherever a face will be filed or turned. Old patternmakers kept a "shrink rule" for each metal, its marks spaced slightly wide.
  • Fillets and even walls. Round every inside corner (radius at least a quarter of the wall thickness) with warm wax pressed in: sharp corners crack as the metal cools (hot tears). Keep walls the same thickness, or change thickness gradually, so no thick lump is cut off from the riser by a thin part that froze first.
  • Split patterns. A wheel, pulley or cylinder is easiest as two half-patterns, one per half of the flask, lined up by two small dowels.
  • Finish. Sand it smooth and seal it with beeswax or linseed oil so it does not swell with damp. A rough pattern makes a rough casting.

Cores. A core is a separate lump of baked sand placed in the mould to make a hole or hollow — the bore of a pipe, the inside of a pot. The pattern carries extra stubs called core prints that leave sockets in the sand; the ends of the core rest in these sockets.

To make a core, pack sand into a wooden core box (a hollow the shape of the core), and bind it with one of these:

  • Oil sand: 40 parts dry sharp sand to 1 part linseed oil (see Oils and Pressing), mixed well. Bake at 200–230 °C (a slow oven, or until a pine shaving laid beside it turns brown) for 1–3 hours, until it is hard and dark brown right through.
  • Flour or dung sand: sand mixed with 1 part in 20 of flour paste, molasses water or fresh dung, dried and baked the same way.

A good core is strong enough to handle but crumbles easily when you knock it out of the finished casting. Poke a thin vent hole along its middle so its gases can escape through the core prints.

Method 1: Green-sand moulding in a flask

"Green" sand simply means damp sand, used as it is, not baked. This is the most useful method in this book: quick, cheap, and the sand is used over and over.

Making the flask

The flask is a bottomless wooden box in two halves that stack: the lower drag and the upper cope. Make each from boards 2–2.5 cm thick into a frame about 30 × 25 cm inside and 8–10 cm deep — enough to leave at least 3 cm of sand between the pattern and every wall. Two pegs on the drag slide into holes on the cope so the halves always meet in the same place. Thin strips nailed inside the walls stop the sand sliding out. You also need two flat moulding boards a little bigger than the flask.

Cruciblelip close to basin Pouring basinkeep it full Spruetapered Parting linedusted Runner, gatenarrow at cavity Riserover the thickest part; feeds it as it shrinks Weights3 × the metal's weight Ventslet air and steam out Copetop half of the flask Cavitybecomes the casting Dragrammed moulding sand Dry sand bednever wet ground
Fig. 1 A green-sand mould ready to pour, in cross-section. Metal runs down the sprue, along the runner and through the gate into the cavity; the riser above the thick part feeds it as it shrinks.

Step by step

  1. Prepare the sand. Riddle it, temper it with water until it passes the squeeze test, and turn it over with a shovel until it is even and lump-free.
  2. Start the drag. Lay the drag upside down on a moulding board. Set the pattern (or the flat half of a split pattern) flat face down in the middle and dust it with parting dust. Riddle 2–3 cm of fine facing sand over it and press it round the pattern with your fingers.
  3. Ram. Shovel in 5–8 cm of loose sand and ram it, first with the wedge end round the edges and pattern, then with the flat end. Ram firmly but not rock-hard: the sand should take a thumbprint only with a hard push. Too soft and the metal pushes the walls out; too hard and steam cannot escape. Repeat layer by layer until the drag is heaped full.
  4. Strike off level with a straight stick. Vent: push a 3 mm wire in every 3–4 cm, to within 1 cm of the pattern.
  5. Roll over. Put the second board on top, grip both boards and turn the drag over. Lift off the top board: the flat face of the pattern lies in smooth sand.
  6. Parting. Smooth the sand and sprinkle parting dust over it so the two halves will not stick. Fit the top half of a split pattern now.
  7. Sprue and riser pins. Put the cope on. Stand a tapered pin 2–3 cm thick upright 3–5 cm beside the pattern (the sprue), and a thicker pin — at least as thick as the thickest part of the casting — right on top of that thickest part (the riser).
  8. Ram the cope the same way, facing sand first. Strike off, vent, wiggle the pins out, and carve a funnel-shaped pouring basin 5–6 cm across at the top of the sprue.
  9. Open and draw the pattern. Lift the cope straight off. Wet the sand at the pattern's edge with a feather so it will not crumble. Drive a small spike into the pattern, tap it lightly in all directions to loosen the pattern by a hair, and lift it straight up.
  10. Cut the runner and gate. In the drag, cut a channel about 1.5 cm wide and 1 cm deep from below the sprue to the cavity, narrowing to a gate about 1 × 0.5 cm where it enters. Mend broken edges with damp sand, blow out loose grains, and set any core in its prints.
  11. Close and weight. Lower the cope back on its pins and set the flask on dry sand. Load the cope with stones weighing at least three times the metal you will pour: liquid metal pushes upward hard enough to float the cope off.
  12. Pour (below), then wait until the casting has set — a few minutes for tin, 15–30 minutes for a hand-sized bronze casting, an hour or more for heavy work.
  13. Shake out. Dump the sand, knock it off the casting, and saw off the sprue, runner and riser for remelting. Break up the burnt sand, sieve out metal bits, and temper it again; it is used over and over.
1 Ram the dragpattern face downon the board 2 Roll it overdust with partingpowder 3 Ram the copearound sprue andriser pins 4 Open itdraw the pattern,cut the gate 5 Close, pourweight the cope,pour without stopping
Fig. 2 Ramming up a two-part sand mould, in five steps.

Tip Make several at once. Once you have a good pattern and a rhythm, two people can ram a small mould in 15–20 minutes. Make a row of moulds before you light the furnace, and pour them all from one melt.

Bells and big round things — cauldrons, pump cylinders — were made without any pattern, by sweeping loam (clay with sand, dung and chopped straw) with a wooden profile board, a strickle, turning about an upright post. The founder sweeps a dried loam core to the inside shape, builds a "false bell" of loam on it to the thickness of the metal, builds the outer cope over that, then lifts the cope off, breaks away the false bell, lowers the cope back and buries the whole mould in rammed earth to pour. It needs no flask, only patience, and suits any shape that is round about an axis.

Method 2: Lost-wax casting in depth

Lost-wax casting copies any shape you can model in wax, including undercuts, hollow handles, lettering, and thin parts. The basic method is in Bronze. These are the points that make the difference between a lucky casting and a reliable one.

Pouring cupwax cone, open at the top Spruewax rod to the thick part Ventsthin wax rods from high points Chapletsiron pins hold the core Face coat3 coats of fine clay cream Backingclay, sand and straw,2–4 cm thick Wax model3–6 mm thick; becomesthe metal Coreclay, sand and dung;makes the hollow
Fig. 3 A lost-wax mould ready for burnout, in cross-section. The wax model is attached to a sprue and cup; vents lead from the high points; a clay core fills the hollow, held by iron pins.

The wax. Pure beeswax sags in warm weather. Melt 3 parts beeswax with 1 part pine resin in a pot standing in hot water (never over an open flame) for a firmer wax that carves crisply. Keep walls 3–6 mm thick for bronze and brass: thinner walls freeze before they fill; thicker walls waste metal and shrink more.

Hollow castings. For a hollow figure or a socket, first make a core of fine clay, sand and dung (about 1 : 1 : 1), shaped and dried. Build the wax over the core to the right thickness. Push 3–4 iron or copper pins (chaplets) through the wax into the core, leaving their ends sticking out 1–2 cm: when the wax is gone, they will hold the core in place inside the mould.

Sprues and vents. Fix the wax model to a wax sprue rod (1–1.5 cm thick for small work, 2 cm for anything over 500 g) that joins the thickest part of the model, so that the metal fills the thin parts last and the thick part is fed. End the rod in a wax pouring cup. Run thin wax rods (3–5 mm) as vents from every high point and every pointed end of the model to the outside of the mould, so no air is trapped. A model with many parts — say six rings — can share one sprue as branches of a "tree".

The investment. The mould material round the wax is called the investment.

  1. Face coat. Mix the finest clay you have (sieve it through a tight cloth) with water to thick cream, and stir in finely powdered charcoal or grog — about one part in four. Paint it on with a soft brush or feather, getting into every crease. Let each coat dry before the next. Three coats, 2–3 mm in total.
  2. Backing. Then pack on 2–4 cm of coarser clay mixed with an equal volume of sand or grog and plenty of chopped straw or dung. The straw burns out, leaving fine channels that let gases escape.
  3. Drying. Dry slowly in the shade for 3–7 days. A thick mould dried too fast cracks.

Burnout. Set the mould cup-down on two stones over a small fire. Let the wax melt and run out into a dish of water — you will get most of it back. Then bury the mould in a bonfire or put it in a The Kiln and raise it gradually to a dull red heat (600–700 °C) over 3–4 hours, and hold it there for an hour. Any black soot left inside the cup must burn away. The mould is ready when you look into the cup and see a clean dull-red glow, with no smoke.

Pouring. Pour while the mould is still red-hot — within a few minutes of taking it out of the fire. Stand it cup-up, buried to its shoulders in dry sand. A hot mould lets the metal fill thin parts before it freezes.

Breaking out. After half an hour, break the investment away, pull the chaplets and plug their holes with hammered pins of the same metal, and dig out the core.

Cuttlefish casting is a quick shortcut for small things in tin, pewter, silver or gold. Rub two halves of a cuttlefish bone flat on a stone, press your model between them, take it out, carve a pouring funnel and a fine vent, tie the halves together and pour. Each bone gives one casting.

Pouring

  1. Lay out the path. The moulds stand on dry sand, close to the furnace, with a clear path between. No water within several metres. Everyone knows where to stand.
  2. Melt under a cover. Keep a layer of charcoal on the melt (see Copper Smelting). Bring the metal to the pouring temperature in the table — a little hotter for thin castings, a little cooler for thick ones.
  3. Skim. Push the dross back with a dry stick or a preheated iron skimmer just before pouring.
  4. Pour in one go. Hold the lip of the crucible close to the pouring basin (a long fall splashes and traps air). Pour fast enough to keep the basin full and do not stop until metal rises in the riser and vents. Pausing halfway makes a cold shut — a seam where two fronts of metal met but did not fuse.
  5. Top up. As the casting sets, the level in the riser sinks. Pour a little more hot metal into it if you can.
  6. Leave it alone. Do not move the mould until the metal in the riser has set hard.

How to tell it worked

  • Complete shape. Sharp corners, all thin parts filled, lettering readable.
  • Sound metal. Saw through a riser or a scrap casting: the cut face should be solid, with no holes. A sound casting rings when tapped; a cracked or holed one sounds dull.
  • Clean surface. Smooth, with sand grains only in odd spots that file off.
  • Weight. A casting that weighs much less than the same volume of metal should (densities in Materials Data Tables) has a hidden hole.

Note Troubleshooting — the common faults. Thin parts missing, rounded edges (misrun) → metal too cold, mould too cold, or poured too slowly. Pour hotter and faster; preheat; make the gate bigger. A seam or crease where metal did not fuse (cold shut) → pour stopped or slowed. Pour in one continuous stream; add a second gate on the far side. A hollow or sunken spot in the thickest part (shrinkage) → no riser, riser too small or on the wrong spot. Put a bigger riser right on the thick part, and gate into it. Round, smooth-walled bubbles (gas holes, blowholes) → sand too wet, not vented, or rammed too hard; damp lost-wax mould; or gas dissolved in the metal. Dry the sand, vent more, ram less hard, keep charcoal on the melt, don't overheat. Rough, lumpy surface with sand stuck in it → sand too coarse, rammed too soft, or metal too hot. Use finer facing sand and dust the cavity with charcoal. Casting is thicker than planned, or bulges → soft ramming let the metal push the sand back. Ram harder. Thin fins of metal along the joint (flash) → cope not weighted or the flask halves did not sit flat. Top half shifted sideways from bottom half → loose guide pins. Make them fit snugly. Cracks at inside corners (hot tear) → sharp corner, or a core too hard to give as the metal shrank. Add fillets; make cores weaker.

Dangers

Danger Molten metal and water explode. A cupful of water under molten bronze turns instantly to steam well over a thousand times its volume and throws metal out in a burning spray. Pour only over dry sand, never on concrete or stone that may hold damp, never in the rain. Preheat every tool that touches the metal — skimmers, stirring rods, extra metal you add — until it is too hot to touch. Never drop cold, damp scrap into a melt. Sand moulds must be vented and only damp, never wet.

Danger Spills and burns. Wear leather shoes or boots (never bare feet or sandals), long sleeves of wool or linen (never anything that melts), and a leather apron. Trousers go over boots, not tucked in, so metal cannot run inside. Practise the whole pour with an empty crucible first. If a crucible cracks, let it fall — never try to catch it.

  • Fumes. Brass gives off white zinc smoke that causes a fever (see Zinc and Brass); lead gives a poisonous fume (see Lead). Pour outdoors, upwind.
  • Lifting. 10 kg of metal needs two people and a shank. Spills come from tired arms.
  • Eyes. Never lean over the mould as you pour: a gas burst comes straight up the sprue.

Going further

With a few good patterns you can make the parts of a The Lathe, and with a lathe you can turn better patterns — the start of Machine Tools and Precision and Interchangeable Parts. Bronze bushings for Bearings and Lubrication, gear blanks for Gears and clocks, and pump barrels for the Pumps are all castings. Type for Printing is cast in a small hand mould in exactly this way. When you can build a tall furnace with a water-driven blast, the same sand moulds take The Blast Furnace and Cast Iron — and cast iron is how pots, stoves, rails and engine frames were made by the million.

How it was first done

The first castings were made in simple open moulds of stone and clay soon after people learned to melt copper, in the Near East in the 5th millennium BC. Lost-wax casting is nearly as old: a small wheel-shaped copper amulet from Mehrgarh, in what is now Pakistan, made around 4,000 BC, is one of the earliest known lost-wax castings, and the astonishing hoard of copper maceheads and crowns found in a cave at Nahal Mishmar, in the Judean desert, was cast by lost wax in the 4th millennium BC. Bronze Age smiths across Europe and Asia cast in two-piece stone and clay moulds; in China, Shang founders (about 1,600–1,050 BC) assembled huge bronze vessels from clay piece moulds fitted around a core.

Casting in sand came much later. The Italian Vannoccio Biringuccio described sand moulds in wooden frames in his book De la pirotechnia (1540), alongside bell-founding in loam with a strickle — the method bell founders still use. In 1707 the English ironmaster Abraham Darby patented a way of casting thin iron pots in sand moulds, which helped make cast iron cheap enough for every kitchen and, later, for the machines of the Industrial Revolution.