Part 8 · Chemistry
Soda Ash and Baking Soda
Soda — sodium carbonate — is the alkali that glass, hard soap, paper and laundry want most. Scrape it from the shores of desert soda lakes, burn it out of salt-marsh plants, or make it from salt, sulfuric acid, limestone and charcoal by the Leblanc process. Bubble carbon dioxide through it and you have baking soda.
- Difficulty
- ●●●●●
- Time
- Days to gather and refine lake or plant soda; a week of furnace work for a batch of Leblanc soda; a day for baking soda
- Steps from zero
- 12 prerequisites →
The full path from nothing — 12 steps before this one
- Fire
- Finding and Preparing Clay
- Sulfur
- Pottery
- The Kiln
- Charcoal
- Lime
- Salt
- Lye and Potash
- Glass
- Saltpeter
- Sulfuric Acid
- Soda Ash and Baking Soda
Do them roughly in this order. See it on the tech tree →
Why it matters
Potash from wood ash (Lye and Potash) is a fine alkali, but it is scarce — a whole winter's fires make a few kilograms — and it soaks up water from the air until it turns to liquid. Soda (sodium carbonate) does the same jobs, and better:
- Glass. The best, clearest, easiest-working glass is soda-lime glass: about 35 parts soda to 100 of sand (Glass, Window Glass).
- Hard soap. Soda lye makes hard bars in one step, without salting out (Soap).
- Paper. Boiling straw, rags or wood in soda lye frees the fibres for pulp (Paper).
- Washing. Washing soda softens hard water, cuts grease, scours wool and cleans pots (Laundry and Bleaching Cloth, Personal Hygiene, Wool).
- Caustic soda. Boiled with slaked lime, soda becomes caustic soda — the strongest common alkali, for soap, paper and chemistry.
- Baking soda — sodium bicarbonate — raises bread and cakes without yeast, settles an acid stomach, and smothers small grease fires.
Soda can be made from common salt, which is almost unlimited. Turning salt into soda was the first great problem of the chemical industry, and solving it in the 1790s created that industry.
How it works
Soda is a carbonate, like potash and limestone: it fizzes with acids and is a base (Acids, Bases and Testing). It comes in three forms:
| Form | What it is | Looks like |
|---|---|---|
| Washing soda (soda crystals) | Soda with 10 parts water locked in its crystals — 63 % water by weight | Large clear crystals that turn into white powder in dry air |
| Soda ash | Dry soda, water driven off by heat | White powder or lumps |
| Baking soda | Sodium bicarbonate — soda that has taken up extra carbon dioxide | Fine white powder, mildly alkaline |
Soda has one very useful habit: it dissolves much more in warm water than in cold. At 0 °C a litre of water holds only about 70 g; at 30–35 °C, about 400–490 g. Common salt dissolves about the same at any temperature. So a warm, strong solution of soda and salt, cooled to near freezing, drops most of its soda as crystals and keeps the salt dissolved — exactly as with Saltpeter.
Why salt needs a detour
Salt is sodium chloride. You want sodium carbonate. Sodium holds chlorine too tightly to swap it directly for carbonate. The Leblanc process does it in two steps:
- Salt + sulfuric acid → saltcake (sodium sulfate) + hydrogen chloride gas (Hydrochloric Acid).
- Saltcake + limestone + charcoal, roasted together at about 1,000 °C → black ash, a mixture of soda and calcium sulfide. The charcoal strips the oxygen from the sulfate, and the limestone takes the sulfur and gives its carbonate to the sodium.
Water then dissolves the soda out of the black ash and leaves the calcium sulfide behind.
The later Solvay process reaches the same goal more cleanly with ammonia, salt water and carbon dioxide (see Going further).
What you need
| Route | Materials | Equipment |
|---|---|---|
| Lake soda | Natron crust or trona from a soda lake | Leaching barrel (Lye and Potash), boiling pot, shallow crystallising trays |
| Plant soda | Dried glasswort, saltwort or seaweed | A burning pit, leaching barrel, boiling pot |
| Leblanc soda (per batch) | 10 kg salt; about 12 kg sulfuric acid at 70 % (Sulfuric Acid); 12 kg crushed limestone or chalk; 6 kg charcoal | Stoneware or iron pan; a small reverberatory furnace or brick hearth reaching bright orange heat with Bellows; iron rake; leaching vats; boiling pan |
| Baking soda | Washing soda; carbon dioxide from limestone and acid, or from a fermenting vat | A tall glass or stoneware jar, glass or clay tubing, a cloth filter |
Where to find it
- Soda lakes. In dry country, lakes with no outlet slowly collect soda from weathering volcanic and granite rocks. Their shores carry white to grey crusts that are slippery-soapy when wet. Famous sources: the Wadi el-Natrun in Egypt (which gave natron its name), Lake Natron and Lake Magadi in East Africa, the shores of Lake Chad (where it is sold as kanwa for cooking), Lake Van in Turkey, the alkaline flats of Hungary, India, Mongolia and northern China, and Owens and Searles Lakes in California. Beneath Wyoming lie the world's largest beds of trona, a natural soda-bicarbonate mineral.
- Telling natron from salt. Natron tastes soapy, bitter and salty all at once; common salt tastes cleanly salty. Natron fizzes with vinegar; salt does not. Natron water turns cabbage juice green (Acids, Bases and Testing); salt water leaves it purple. White crusts that are bitter and cooling but do not fizz are other salts (sulfates) — not soda.
- Salt-marsh plants. Glasswort (Salicornia), saltwort and barilla (Salsola species) — fleshy, jointed, salty-tasting plants of salt marshes, coastal sands and inland salt flats. Their ash can hold a quarter or more of its weight in soda. See Glass.
- Seaweed. The ash of kelp and wrack ("kelp" as sold in the 1700s) holds only a few per cent soda, with much potash, salt and iodine. It was used for soap and glass when nothing better was near.
- Salt for the Leblanc route: see Salt. Limestone and chalk: see Lime. Charcoal: see Charcoal.
Method 1: Refining natural soda
- Gather crust from the lake shore in the dry season, when it is thickest. Leave the muddy layer behind.
- Dissolve it in warm water — about 1 part crust to 2 parts water — in a barrel or large pot, stirring. Let the mud settle for a day.
- Pour off the clear liquid and boil it down until a drop on a cold stone forms crystals.
- Cool it slowly in shallow wooden or clay trays, in the cold of night or in winter. Large, clear, flat crystals of washing soda grow. Pour off the liquid (it holds most of the salt) and drain the crystals.
- For purer soda, redissolve the crystals in the least possible warm water and crystallise again.
- For soda ash, heat the crystals in an iron pan: they melt in their own water, boil, and dry to a white powder. Heat it to a dull red glow to finish. Store dry and sealed.
In cold climates, soda lakes do this by themselves: soda crystallises along the shore in winter and is raked up in spring.
Method 2: Soda from plant ash
- Harvest glasswort or saltwort in late summer, when the stems are fullest. Dry them in heaps for 1–2 weeks.
- Burn them in a pit about 1 m across and 50 cm deep, adding plants slowly so the fire stays hot. Barilla burners kept the fire going for hours until the ash melted together into a hard, grey-blue, stony cake. Seaweed is burned the same way.
- Break up the cooled cake, crush it, and leach it with water exactly like wood ash (Lye and Potash).
- Boil down and crystallise as in Method 1. Expect a mixture of soda and potash, with salt. For glass and soap, the crude salts from simply boiling the lye dry are good enough.
Method 3: The Leblanc process
This is heavy, hot, smelly industrial chemistry. It needs strong Sulfuric Acid, a furnace that reaches bright orange heat, and a team. Make sure you can also capture the hydrogen chloride gas — the first Leblanc works poisoned everything around them.
Stage 1: Saltcake
- In a stoneware jar, or a cast-iron pan if you have one, mix 10 kg salt with about 12 kg of 70 % sulfuric acid (or 9 kg of concentrated acid). It froths and gives off clouds of hydrogen chloride.
- Lead the gas away into absorbers or a wet tower, as in Hydrochloric Acid Method 2. This gives you some 15–20 kg of hydrochloric acid as a by-product.
- When the frothing slows and the mass turns pasty, rake it out onto the hearth of a furnace and roast it at a dull red heat (about 600 °C) for 1–2 hours, stirring, until it stops fuming. What is left is saltcake: a white to greyish, porous solid. About 12 kg.
Stage 2: Black ash
- Crush and mix by weight: 2 parts saltcake, 2 parts limestone or chalk, 1 part charcoal, all broken to the size of peas. For 12 kg of saltcake: 12 kg limestone, 6 kg charcoal.
- Heat it on the hearth of a reverberatory furnace (a furnace where the flame passes over the charge, not through it) or in a large clay crucible in a strongly blown furnace, to a bright orange-yellow heat — about 950–1,000 °C.
- Stir constantly with an iron rake. The charge softens and becomes a thick, pasty, bubbling mass.
- The sign it is done: small, bright jets of flame — the old workers called them "candles" — burst from the surface all over. That is carbon monoxide escaping and burning. Rake the mass out at once; overheating spoils it. For 30 kg of charge, expect 1–2 hours.
- Let it cool into a porous, grey-black cake: black ash.
Stage 3: Leaching
- Crush the black ash to the size of walnuts.
- Leach it like wood ash (Lye and Potash), but with lukewarm water (30–40 °C), and quickly — run it through two or three barrels of black ash in a day. Hot water or long soaking lets the calcium sulfide react back and spoil the soda with yellow sodium sulfide.
- The liquid that runs out is soda liquor, yellow to brown. Let it settle. Blowing air through it, or letting it stand in shallow pans for a day, improves it.
- Boil down in an iron pan. As it thickens, soda separates as a crust of fine crystals; rake it out and drain it. Or cool the strong liquor for washing soda crystals, as in Method 1.
- Calcine the drained soda to a dull red to burn off traces of sulfide and charcoal, giving white soda ash.
Expect very roughly 5–6 kg of soda from 10 kg of salt.
The waste
The insoluble grey sludge left in the barrels — about as heavy as the black ash itself — is mostly calcium sulfide. Wet and exposed to air or acid, it gives off hydrogen sulfide, a gas that smells of rotten eggs and kills. Spread it thin in the open to weather, far from houses and water, or bury it under clay. Never pour acid on it.
Method 4: Baking soda
Baking soda dissolves only about 90 g per litre of cold water — much less than soda. So when carbon dioxide meets a strong soda solution, the baking soda it makes falls out as a white powder.
- Make the solution. Dissolve washing soda crystals in cold rainwater until no more will dissolve — roughly 800–900 g of crystals per litre of water at room temperature. Warm water helps them dissolve; let it cool again before use. Pour it into a tall jar and stand the jar in cold water.
- Make carbon dioxide. In a second jar, put broken limestone, chalk or marble and pour diluted Hydrochloric Acid (about 10 %) or strong vinegar on it through a thistle funnel (Hydrogen, Oxygen and Gases). Do not use sulfuric acid: it coats the stone with gypsum and stops.
- Bubble the gas through a glass or clay tube reaching to the bottom of the soda jar, for several hours. A fermenting vat of beer or wine (Beer, Wine and Cider) also makes plenty of carbon dioxide: lead a tube from its sealed lid.
- White powder gradually settles. When the jar no longer gains powder, stop.
- Filter through a tight cloth, rinse once with a little ice-cold water, and dry at room temperature on a cloth in the shade. Heating it above about 50 °C turns it back towards soda.
The old way: bakers in the 1800s made saleratus by laying potash or soda on trays in a closed box over a fermenting vat for several days, so it slowly soaked up carbon dioxide.
Baking powder
Baking soda raises dough only when it meets an acid: sour milk, buttermilk, yoghurt, honey, lemon juice — or cream of tartar, the white crust that forms inside wine barrels (Beer, Wine and Cider), scraped out, dissolved in boiling water, filtered and crystallised on cooling.
- Baking powder: 1 part baking soda, 2 parts cream of tartar, 1 part dry starch (keeps it dry). Use about 1 heaped teaspoon (5 g) per 100 g of flour.
- With sour milk: about ½ teaspoon (2–3 g) of baking soda per 250 ml of sour milk or buttermilk.
- Too much baking soda tastes soapy and turns the crumb yellow-green.
How to tell it worked
- Fizz test: soda, washing soda and baking soda all fizz strongly with vinegar.
- Soda or potash? Leave a lump in damp air overnight. Potash becomes wet and runny. Soda stays dry, or crumbles to white powder.
- Soda or baking soda? Soda turns cabbage indicator green; baking soda only blue. A spoon of baking soda heated dry in a test tube gives off gas and droplets of water, and what is left is soda.
- Flame test: a pinch of any sodium salt on a wire in a spirit-lamp flame colours it a strong yellow-orange. Potash gives a faint lilac.
- Glass test. The real proof: it melts sand into glass (Glass).
Note Troubleshooting. Lake crust does not fizz → it is a sulfate or salt crust, not soda. Search for crust that does. Few crystals on cooling → the liquid was not strong enough, or not cold enough. Boil down further; cool near freezing. Black ash does not "candle" → not hot enough. More air from the bellows; drier charcoal. Soda liquor yellow and smells of rotten eggs → leached too hot or too long. Use lukewarm water and leach faster; calcine the soda well. No baking soda forms → the soda solution is too weak or too warm, or the gas is mostly air. Make it stronger, cool it, and check that the gas puts out a candle. Washing soda turned to powder in the jar → normal; it has lost water. It is still soda, and stronger by weight.
Dangers
Danger Hydrochloric acid gas in Stage 1 burns eyes and lungs. Work outdoors, catch the gas, and stay upwind. See Hydrochloric Acid.
Danger Hydrogen sulfide from the waste kills. At first it smells strongly of rotten eggs; at deadly levels it numbs your sense of smell, so the smell vanishes just when it is most dangerous. Never put black-ash waste in pits, cellars or closed places, never wet it with acid, and keep it far from houses and wells.
- Caustic. Strong soda solution, and especially caustic soda, burns skin and blinds as lye does (Lye and Potash). Wear eye protection and keep water at hand.
- Furnace work. The black-ash furnace runs at 1,000 °C and spits molten material; wear leather, use long rakes, and keep water away from molten charge.
- Carbon monoxide from the black-ash furnace and carbon dioxide from the gas jar can suffocate in enclosed spaces. Work outdoors.
- Baking soda as medicine: half a teaspoon in a glass of water for occasional heartburn only. Large or frequent doses upset the body's salt balance — dangerous for people with heart or kidney disease.
Going further
The Solvay process (in outline)
The Belgian chemist Ernest Solvay made soda from just salt and limestone, with ammonia as a reusable helper:
- Saturate brine with ammonia gas (Ammonia).
- Pass carbon dioxide (from burning limestone in a Lime kiln) up through it in a tall tower. Baking soda crystallises out, because it is not very soluble in this cold, salty liquid. Filter it off.
- Heat the baking soda to about 200 °C: it gives soda ash, and the carbon dioxide goes back to the tower.
- Add the quicklime from the kiln to the leftover liquid (ammonium chloride): the ammonia is freed and reused. The only waste is calcium chloride solution.
It is clean and cheap, but every step must be gas-tight and the ammonia losses kept tiny, or it fails — many inventors tried before Solvay succeeded. It needs good pumps, towers and pipes (Machine Tools). Until then, use Leblanc or natural soda.
Other uses to grow into
- Caustic soda, made from soda and slaked lime exactly as caustic potash in Lye and Potash, cooks wood into paper pulp (Wood Pulp, Kraft Paper and Paperboard) and makes hard soap quickly.
- Water softening for boilers: a little soda in boiler feed water keeps scale from forming (The Steam Engine).
- Oral rehydration: older World Health Organization rehydration formulas included 2.5 g of baking soda per litre, to correct the acidity that severe diarrhoea causes (Oral Rehydration).
- The standard base for titrations (Acids, Bases and Testing).
How it was first done
Natron from the Wadi el-Natrun was used by the ancient Egyptians to dry bodies for mummification, to clean, and to make glass and faience; the Romans called it nitrum, and our chemical symbol for sodium, Na, comes from its Latin name, natrium. For centuries Europe's glassmakers and soapmakers bought barilla ash from Spain and the Levant, and Scotland and Ireland burned seaweed into kelp.
In 1783 the French Academy offered a prize for making soda from salt. Nicolas Leblanc found the method of this chapter and patented it in 1791, but the Revolution seized his factory, he never received the prize, and he died in poverty in 1806. His process spread through Britain from the 1820s, after the salt tax was lifted, and grew into the first heavy chemical industry — along with the first pollution laws. Ernest Solvay made his ammonia-soda process work in Belgium in the 1860s, and by about 1900 it had replaced Leblanc's almost everywhere. Baking soda was being sold for cooking in the United States by the 1840s; Austin Church and John Dwight began making it in 1846.
Source: content/entries/chemistry/soda-ash.md