Part 1 · Staying Alive
Stone Tools
How to find the right stone and break it into knives, scrapers and hand axes sharper than steel — and how to grind tough stone into an axe that fells trees.
- Difficulty
- ●●●●●
- Time
- Minutes for a sharp flake; an hour or two for a hand axe; days for a ground axe
- Steps from zero
- 0 prerequisites →
You need first
Nothing — start here.This unlocks
Abrasives and Grinding StonesQuarrying and Cutting StoneFarming from SeedHorn and Bone WorkingHunting and TrappingSalvaging from RuinsBasic WoodworkingWhy it matters
Without a cutting edge you cannot butcher meat, scrape a hide, cut cord, sharpen a stick or shape a handle. Stone tools were humanity's only cutting tools for more than three million years — about 99% of our history. A fresh flake of flint or obsidian is sharper than a steel razor.
Stone tools lead to Basic Woodworking, Hunting and Trapping, Hides and Leather, the Bow and Arrow and Farming from Seed. They will carry you all the way until you can smelt Copper Smelting and Iron (the Bloomery) — and even then, flint stays useful for striking sparks (Fire) and as a quick knife.
How it works
Good tool stone is like glass: hard, brittle and the same all the way through, with no grain or crystals to steer a crack. Strike it sharply near an edge and the force spreads into the stone as a cone — like the cone-shaped chip a pebble knocks out of a window. The crack follows that cone and peels away a thin, curved, razor-edged slice called a flake. This shell-like curved break is called conchoidal fracture, and it is the whole secret of knapping (knapping — shaping stone by breaking off flakes).
Three rules control every flake:
- The edge angle must be less than 90°. You strike a surface called the platform. The flake comes off the face that meets the platform. If the angle between them is a right angle or more, nothing will come off except crumbs. Look for edges sharper than a right angle — about 60–80° is ideal.
- Strike close to the edge, and into the stone. Hit 3–6 mm back from the edge. Further in, you remove a thicker flake or nothing; at the very edge, you just crush it. Swing so the blow would pass through the stone at an angle, not glance off it.
- Flakes follow ridges. A flake runs along the stone like water along a gutter, following any ridge on the face below the platform. Use the ridges left by earlier flakes to guide the next one.
What you need
| Tool | What | Size |
|---|---|---|
| Hard hammerstone | A rounded, tough river cobble — quartzite, granite, sandstone, basalt | Egg- to fist-sized; 200 g to 1 kg |
| Soft hammer (billet) | A length of deer or elk antler, or a club of dense hardwood | 20–30 cm long, as thick as your wrist |
| Pressure flaker | The pointed tip of an antler tine, or a pointed bone | 10–15 cm long |
| Abrader | A coarse lump of sandstone | Palm-sized |
| Leg pad | A thick piece of leather or folded bark | To protect your thigh |
| Grinding slab | Flat sandstone, with sand and water | For ground axes |
Where to find it
Tool stone — the best is glassy and fine-grained:
- Flint and chert — hard, waxy-to-glassy, grey, black, brown or banded stone. Flint forms as knobbly nodules in chalk and limestone, often with a white crust (the cortex). Look along chalk cliffs, in fields and riverbeds below chalk country, and on beaches. Chert forms in layers in limestone.
- Obsidian — black or dark glassy volcanic rock. The sharpest edges of all, but brittle. Found in volcanic regions.
- Chalcedony, jasper and agate — waxy, often colourful forms of silica found in volcanic rocks and gravels.
- Quartzite and fine basalt — grainier, tougher and harder to work, but serviceable for big tools.
Testing a stone.
- Look at a fresh break. Knock a corner off. Good stone breaks with smooth, shell-shaped curves and sharp edges. Grainy, sugary or crumbly breaks mean poor stone.
- Listen. Hold the stone loosely and tap it with a hammerstone. A clear ring means it is sound inside; a dull clunk means hidden cracks that will ruin your work.
- Wet it. Licking a surface shows its true texture and colour, and makes cracks and grain easier to see.
- Avoid stones with visible crystals, cracks, white chalky spots inside, or frost-cracked surfaces.
Antler is dropped by deer every winter and can be found on the forest floor in late winter and spring. Dense hardwood (oak, hickory, olive, ironwood) works as a substitute. Hammerstones are rounded cobbles in any riverbed; choose ones that feel heavy for their size.
Stone for ground axes must be tough rather than glassy: dense, fine-grained, dark volcanic rocks such as basalt, dolerite and diorite, or the greenish stones called greenstone and jade. They don't break like glass; they resist shattering. Look for them as dark, heavy cobbles in streams in volcanic or mountain country.
Method 1: Flakes — the first knife
This is the oldest and easiest technique, and gives a usable knife in minutes.
- Sit down, with a leather pad over your thigh. Wear eye protection if you have any (a slit visor of bark helps) — otherwise turn your face away at the moment of striking.
- Choose a core: a fist-sized or bigger nodule with at least one edge sharper than a right angle. If there is none, make one: strike a round nodule hard against a big anvil stone to split it in two. The flat broken face makes a perfect platform.
- Hold the core in your left hand, resting on your thigh, the platform facing up and the face you want the flake to come off facing away from you.
- Strike downward and slightly outward with the hammerstone, 3–6 mm in from the edge, with a firm, snapping, follow-through blow — like cracking a whip, not pushing.
- Collect the flake. A good one is thin, with a sharp edge all round, a smooth inner face with a small bump (the bulb) just below where you struck.
- Repeat, using the ridges left by the first flakes to guide the next ones. One good nodule can give dozens of flakes.
Use the flakes as they are. An unretouched flake is the sharpest knife you will ever own. Use it for butchering, cutting cord and hide, and whittling. When the edge dulls, strike another. For a sturdier scraper, choose a thick flake and nibble its edge into a steeper, stronger angle with small taps.
Blades are special flakes at least twice as long as wide, with parallel edges. Expert knappers strike them in series from a carefully prepared cone-shaped core. They give the most cutting edge from the least stone, but they take a great deal of practice.
Method 2: The hand axe
The hand axe (or biface, because it is worked on both faces) is a general-purpose heavy tool: for chopping wood and bone, digging, and butchering large animals. It is held in the hand, not hafted.
- Choose a blank: a flat, oval nodule or a big thick flake, about 15–20 cm long and less than 6 cm thick.
- Make an edge. Work around the rim with the hard hammerstone, striking a flake off one face, then turning the stone over and striking the next flake from the scar of the first — alternating faces. This creates a zig-zag edge running all round, and the stone gets thinner as you go.
- Thin it with the soft antler or hardwood billet. A soft hammer gives longer, flatter, thinner flakes that run across the face towards the middle. Before each strike, grind the edge where you will hit a few strokes with the sandstone abrader. This strengthens the platform so it does not crumble.
- Aim for the shape: a teardrop or oval, pointed at one end, about 12–18 cm long and 3–5 cm thick. A good one is at least three times as wide as it is thick.
- Straighten the edge with small, careful blows so it runs in a straight line when seen from the side, rather than snaking.
- Blunt the butt — the part your palm grips — by grinding it on the abrader, so it does not cut your hand.
Tip Mistakes to expect. The commonest is a step fracture: the flake stops short with a square ledge. It happens when the blow is too weak or too steep. Remove it from the other side, or work around it. If the stone snaps in two, you hit too hard in the middle of a thin piece. Every knapper breaks many stones; it is part of learning.
Method 3: Pressure flaking
For fine work — sharpening an edge, making serrations, shaping arrowheads (Bow and Arrow) — you press flakes off instead of striking them.
- Hold the piece on a leather pad in the palm of your left hand, the edge facing outward and your fingers supporting the face below it.
- Put the tip of the antler flaker on the edge, slightly onto its underside, with the edge abraded first.
- Press in (towards the middle of the stone) and down firmly and steadily, then give a small extra push. A thin flake 5–15 mm long pops off the underside.
- Work along the edge in a row, then turn the piece over and work the other side.
Method 4: The ground stone axe
Flaked flint axes are sharp but chip easily on hard wood. A ground axe of tough stone keeps its edge through hours of chopping. Making one is slow, steady work rather than skilled work.
- Choose a cobble of basalt, greenstone or similar, close to the shape you want: elongated, 12–20 cm long.
- Peck it to shape. Strike it over and over with a hard quartzite hammerstone, in light rapid blows. Each blow crushes a tiny pit. Thousands of blows slowly reduce the surface. Expect 5–15 hours.
- Grind the edge. Wet a flat sandstone slab, sprinkle on sand, and rub the axe back and forth along the slab, pressing hard. Keep it wet. Grind both faces to meet at an edge of about 40–60°. Expect several more hours; the slab gradually develops a dished hollow.
- Polish the whole body if you have time; a smooth axe is less likely to crack and sits more firmly in its handle.
Hafting: adding a handle
A handle multiplies the force of a blade and keeps your fingers away from the edge. See Basic Woodworking for making handles.
- Knife: split the end of a hardwood stick 4–5 cm down. Slip the blade's base into the split. Bind tightly with wet sinew or Cordage and Rope. Sinew shrinks as it dries and grips like a vice.
- Glue: melt pine or spruce resin gently beside a fire (not in it), and stir in powdered Charcoal — about 1 part charcoal to 3 or 4 parts resin — plus a pinch of dry dung or a little fat or beeswax so it is less brittle. Apply hot to the joint and over the binding. See Tar, Pitch and Glue for birch tar, a stronger glue, and Glues and Adhesives for the rest.
- Axe: carve a club of hardwood with a thickened head. Burn and gouge a tapering hole through the head, slightly smaller than the axe's butt. Drive the axe head in, sharp end out, so each blow wedges it tighter. Leave a hand's width of wood around the hole so the handle does not split.
- Grind the parts of the blade that touch the lashing, so the sharp edges don't cut the binding.
How to tell it worked
- A good flake shaves hair from your arm, and slices cleanly through a hide or a bundle of grass.
- A good hand axe is symmetrical, thin, and chops a wrist-thick green branch in a few dozen strokes.
- A good ground axe has a smooth, even edge with no chips, and cuts into green wood leaving a clean, shiny cut rather than a crushed one.
Note Troubleshooting. Only crumbs come off → the edge angle is too steep (90° or more); find or make a sharper edge. Flakes stop short with a step → strike harder and further through the stone, or use a soft hammer. The platform crushes → grind it with the abrader before striking. The stone snaps across → the piece is too thin for that blow; use lighter blows or pressure flaking. Stone won't flake cleanly at all → it is grainy or full of cracks; find better stone. Many knappers improve chert by burying it in sand under a fire and heating it slowly, for most of a day, to about 250–350 °C, holding it there for a few hours, then letting it cool overnight under the ashes. Heated chert turns glossier and flakes more easily — but heated too fast it shatters.
Dangers
Danger Eyes and tendons. Tiny flying chips of flint and obsidian can blind you. Turn your face away or shield your eyes, and never knap near other people's faces. Flakes cut deeply and easily — a slip can sever a tendon in a finger or wrist. Work over a pad, never in your lap without one, and keep your holding hand padded.
- Dust. The fine powder from knapping and grinding flint, chert and quartzite contains silica. Breathed in, day after day for years, it scars the lungs (silicosis). Work outdoors, in a breeze, and do not sweep up dust dry.
- Debris. Knapping leaves razor-sharp waste. Work in one place, on a hide you can carry away, and bury the waste. Don't knap where people walk barefoot.
- Hammer hits. Hitting your own fingers is common. Grip the core so your fingers are behind it, not under the blow.
What this unlocks
With stone tools you can cut and shape wood (Basic Woodworking), make spears and traps (Hunting and Trapping), skin animals and scrape hides (Hides and Leather), and clear land for Farming from Seed. Ground stone axes make felling trees and building houses (Shelter) practical. Later, stone working grows into Quarrying and Cutting Stone, millstones (Grain, Flour and Bread) and, eventually, into metal tools (Copper Smelting, Bronze, Iron (the Bloomery)).
How it was first done
The oldest known stone tools were found at Lomekwi in Kenya and are about 3.3 million years old — older than our own genus. Simple core-and-flake tools (called Oldowan) appear in Ethiopia about 2.6 million years ago. The teardrop-shaped hand axe appeared in East Africa around 1.7 million years ago and was made, almost unchanged, for more than a million years across Africa, Europe and Asia. Deliberately heat-treated stone appears in South Africa about 160,000 years ago, and pressure flaking by about 75,000 years ago. Edge-ground axes were made in northern Australia more than 40,000 years ago, and polished stone axes became the essential tool of the first farmers, who cleared Europe's forests with them from about 7,000 years ago.
Source: content/entries/survival/stone-tools.md