◆ Rebuild

Part 5 · Cloth and Clothing

Wool

Shear or pluck the fleece from sheep (or comb the soft undercoat from goats, camels and alpacas), sort it, wash out the grease without felting it, and card or comb it ready to spin. Wool is the warmest fibre there is — it keeps you warm even when it is wet.

Difficulty
●●●●●
Time
10–30 minutes to shear a sheep by hand; a day to wash a fleece and a week to dry it; an hour to card enough for an evening of spinning
Steps from zero
3 prerequisites →

You need first

Keeping Animals

This unlocks

Felt
The full path from nothing — 3 steps before this one
  1. Stone Tools
  2. Farming from Seed
  3. Keeping Animals
  4. Wool

Do them roughly in this order. See it on the tech tree →

Why it matters

In a cold or wet climate, wool is the difference between life and death. A woollen garment stays warm when soaked by rain or sweat, because the fibres resist wetting and hold air between them even when damp. Wool is also springy, so cloth made from it keeps its shape and its warmth for years; it burns poorly and puts itself out, which makes it the safest cloth near a fire or furnace (Glass, The Kiln); and it takes dye beautifully (Dyes and Mordants).

Better still, wool grows back. A sheep gives a new fleece every year for ten years, eating nothing but grass you could not eat yourself. From wool come yarn and cloth (Spinning and Weaving Cloth), Knitting, Crochet and Netting, Felt (which needs no spinning at all), blankets, tents, socks (Footwear) and the warm layers of Making Clothes. Its grease, lanolin, softens leather and skin.

How it works

A wool fibre is not a smooth hair. Under a microscope its surface is covered in tiny overlapping scales, like roof tiles. These scales let fibres slide one way past each other but not back. Rub wet, warm wool with soap and the fibres creep along and lock together permanently: this is felting. It is wonderful when you want Felt, and a disaster when you are trying to wash a fleece.

Most wool fibres are also crimped — wavy along their length. Crimp makes the fibres push apart and trap air, which is why wool is warm and springy. Fine wool has small, tight crimp; coarse wool has big, loose waves or none.

A raw fleece is not just fibre. It carries:

  • Lanolin (wool grease) — a waxy fat made by the sheep's skin. It is solid at room temperature and melts at about 40 °C. Wool can be 10–25 % grease by weight; fine-wool sheep have the most.
  • Suint — dried sweat. Unlike lanolin, suint dissolves in plain cold water, and it is itself a mild natural soap.
  • Dirt, dung, seeds and burrs.

Washing a fleece (scouring) means getting the lanolin out with hot water and a mild cleaner without the agitation and sudden temperature changes that make it felt. After scouring, the fibres are untangled and laid out evenly by carding (for soft, airy yarn) or combing (for smooth, strong yarn).

What you need

Item Notes
Sheep (or goats, camels, alpacas, llamas, yaks, angora rabbits) See Keeping Animals and Animal Health
Shears Iron or steel blade shears: two blades on one springy U-shaped bow, about 30 cm long. See Scissors, Shears and Folding Knives. Before shears, wool was plucked by hand
Skirting table A frame of slats or a net, about 1.5 × 1 m, raised to waist height, so dirt and short bits fall through
Tubs Wooden or clay tubs or large pots for washing (Pottery, Barrels and Cooperage); a way to heat water to 60–70 °C
Cleaner Soap, soapwort, or stale urine. Not strong Lye and Potash
Drying rack A net, a slatted frame or clean grass, in shade with a breeze
Hand cards Two paddles set with bent wire teeth — see below
Wool combs Two combs with long, tapering teeth, for smooth worsted yarn — see below

A fleece weighs about 1–2 kg from a small primitive sheep and 2–5 kg from a larger farm sheep. It loses a third to half of that weight in washing.

Where to find it

  • Sheep. Domestic sheep descend from the wild mouflon of the mountains from Turkey to Iran. Wild sheep have a coat of coarse hair over a short woolly undercoat that falls out in spring; thousands of years of keeping the woolliest animals gave the domestic fleece. In a ruined world, feral sheep survive on hills, islands and abandoned farms. Small, hardy, often brown breeds that shed their fleece in late spring (Soay, Shetland, Icelandic and many "unimproved" island and mountain breeds) are the easiest to keep without shears.
  • Goats. All goats in cold climates grow a fine, soft down (cashmere) under their coarse outer hair; it loosens in spring and can be combed out, about 100–300 g per goat. Angora goats grow long, shiny curls (mohair) that are sheared twice a year.
  • Camels, yaks, alpacas and llamas. Camels and yaks shed a soft brown down in spring that can be gathered by hand or combed out. Alpacas and llamas are sheared every one or two years; their fibre has almost no grease and washes easily in plain warm water.
  • Angora rabbits give very soft, fluffy fibre, plucked or clipped every three months.
  • Soapwort (Saponaria officinalis) is a pink-flowered plant of roadsides, river banks and old gardens in Europe and western Asia, 30–90 cm tall, with smooth oval leaves in pairs and clusters of five-petalled pink or white flowers with a clove scent. Its roots and leaves foam when crushed and rubbed in water. Soapnuts (the fruit of Sapindus trees in warm climates) and the bark of soapbark (Quillaja) work the same way.

Step by step

1. Shear (or pluck) the fleece

Shear in late spring or early summer, when the weather has warmed and the new growth has "risen" — a soft band of new wool appears next to the skin, and the old fleece parts easily along it. Never shear just before cold, wet weather; a freshly shorn sheep can die of cold.

  1. Starve the sheep for 6–12 hours beforehand (water only): a full gut makes the sheep uncomfortable when tipped over and soils the fleece.
  2. Work on a clean floor — swept boards, a tarp of old sacking, or clean grass.
  3. Tip the sheep onto its rump, sitting it between your knees with its back against your legs. A sheep in this position stops struggling.
  4. Shear in long strokes close to the skin, with the blade points angled slightly away from the skin and the skin stretched flat with your other hand. Start with the belly (keep it apart — it is dirty), then the inside of the back legs, then open the neck and work round and along the sides and back in long sweeps. Try to take the fleece off in one piece, like peeling a coat.
  5. Never cut twice. Going back over a patch makes short "second cuts" that spoil the yarn.
  6. Watch for skin folds around the legs, the udder or teats and the face. Treat any nicks at once (see Dangers).

Rooing (plucking). With a breed that sheds, wait until the fleece lifts away at the rise in late spring, and simply pull it off by hand in handfuls, or comb it out. It does not hurt the sheep when the fleece is ready. If it resists, wait a week. This is how wool was gathered for thousands of years before shears.

2. Skirt and sort

Shoulders NECK Back Britch finest, most even weathered coarsest TAIL Skirtingsdirty edges, belly, legs — pull off Sidesgood, even wool ONE STAPLE (LOCK) Tipweathered, oftendarker and brittle Crimpsmall, tight waves= fine, warm wool Cut endnext to the skin 5–25 cm
Fig. 1 A fleece laid out cut-side down. The best wool is on the shoulders and sides; the edges, belly and back legs are skirted off. Below: one staple (lock) of wool, showing crimp and the weathered tip.
  1. Throw the fleece out flat on the skirting table, cut side down, like a rug.
  2. Skirt it: pull off the dirty edges — dung-caked locks ("dags"), the belly wool, the short coarse wool of the lower legs, and anything full of burrs and seeds. Use these for felt, stuffing or compost.
  3. Sort it: the finest, most even wool is usually on the shoulders and upper sides; it becomes coarser along the back, and the coarsest is on the britch (the hindquarters). Keep these grades in separate bags if you want an even yarn.
  4. Check soundness: take one lock (staple) and flick it hard between your hands, near your ear. Good wool "pings" and holds. If it snaps in the middle, the sheep was ill or starved at that point in the year: that wool is only good for felt.
  5. Note the staple length: short, fine, crimpy wool (5–10 cm) suits carding and soft woollen yarn; long wool (10–25 cm) suits combing and smooth worsted yarn.

Store raw fleece in cloth bags or baskets, not sealed pots — it sweats and rots. Wash it within a few months; old grease sets hard and will not wash out.

3. Wash out the grease (scouring)

Do this in batches of about 500 g–1 kg of fleece. Handle wool like an egg: no rubbing, no stirring, no sudden temperature changes.

  1. Cold soak (optional, but it helps). Soak the fleece overnight or for a few days in cold rain or river water. The suint dissolves and lifts out much of the dirt. Lift the wool out and let it drain; throw the brown water on the garden (Compost and Manure) — it is rich in potash.
  2. Heat the wash water to 60–70 °C — too hot to hold your hand in for more than a second or two, but well below boiling, with no bubbles. Lanolin melts and washes out only above about 50 °C, so cool water will not do.
  3. Add the cleaner, then the wool — never the other way round:
    • Soap: about one cupful of soft soap per large tub (20–30 litres), dissolved before the wool goes in.
    • Soapwort: chop and boil a double handful of roots and leaves in water for 15 minutes, strain, and add the frothy liquid.
    • Stale urine: the traditional scour. Urine left a week or two turns to ammonia, which turns grease into soap. Use 1 part stale urine to 3–4 parts hot water.
  4. Push the wool gently under and leave it for 15–20 minutes. Do not stir. If the water cools below about 50 °C, the grease sets back on the wool: lift the wool out before that.
  5. Lift it out, let it drain, and squeeze gently — do not wring.
  6. Repeat with fresh hot soapy water until the water stays fairly clear: usually twice for coarse wool, three times for greasy fine wool.
  7. Rinse twice in clean water at the same temperature as the last wash.
  8. Spin out the water: put the wool in a cloth bag or net and swing it round your head outdoors, or roll it in a cloth and press.
  9. Dry spread thin on a net or clean grass, in the shade with a breeze, turning it daily. It takes 1–3 days in summer.

Warning Strong lye destroys wool. Wool is a protein, like hair and skin, and caustic lye dissolves it — that is how drain cleaner works on hair. If you must use wood-ash lye, use only a very weak, slippery-but-not-burning solution, and rinse thoroughly. Soap, soapwort and stale urine are far safer.

Recovering lanolin. Let the first hot wash water cool overnight. A grey, greasy layer forms on top: skim it off, melt it in fresh hot water, and let it set again to clean it. Lanolin softens chapped skin, dresses leather (Hides and Leather), waterproofs wool, and is a base for ointments (Making Medicines).

Not scouring at all. Some spinners spin wool "in the grease" (unwashed, or only cold-soaked) and wash the finished yarn or cloth instead. It is faster and the lanolin makes spinning smooth, but the yarn smells of sheep until washed.

4. Open the locks

Before carding, open each lock by pulling the fibres gently apart with your fingers (teasing), shaking out seeds and dirt as you go. For long wools, hold a lock by its cut end and tap or brush its tip with a single comb (a flick carder — a small paddle with bent teeth) to open it.

5. Card it (for woollen yarn)

CARDING — 1. BRUSH top card brushes lightly across the loaded card,only the tips of the wire teeth touching Hand cards20 × 10 cm, bent wire teeth CARDING — 2. ROLL A ROLAG lift the airy sheet off the card and roll itacross the fibres into a loose sausage carded sheet Rolag→ woollen yarn COMBING — 3. COMB fixed comb, longiron or bone teeth swing COMBING — 4. DRAW OFF Topparallel fibres → worsted short "noils" stay on the comb
Fig. 2 Carding and combing. Carding mixes the fibres into a soft, airy roll for warm woollen yarn; combing lines them up parallel for smooth, strong worsted yarn.

Hand cards are two flat wooden paddles, each about 20 × 10 cm with a handle, faced with a sheet of stiff leather pierced by many short teeth of bent wire. The teeth (about 1–1.5 cm long, 3–5 mm apart in rows) all lean slightly towards the handle. Making the teeth needs drawn wire (Copper Wire explains drawing wire; iron wire is drawn the same way). Before wire, wool was teased by hand, combed, or beaten loose with a vibrating bowstring, as is done for Cotton.

  1. Load: hold one card on your knee, teeth up, handle away from you. Lay a few teased locks across the teeth and pull them so they catch, until the card is thinly and evenly covered. Overloading is the commonest mistake.
  2. Card: hold the second card in your other hand, teeth down, handle towards you. Brush it lightly across the first card, 5–10 strokes, with only the tips of the teeth touching. The fibres transfer and straighten.
  3. Transfer: reverse the top card so its tip faces the tip of the loaded card, and push it back so all the fibre moves onto one card. Card again. Two or three transfers are usually enough.
  4. Roll a rolag: lift the fibre off the card in one airy sheet and roll it loosely across the fibres into a sausage about the length of the card. Spinning from the end of a rolag gives woollen yarn: light, fuzzy, very warm.

6. Comb it (for worsted yarn)

Wool combs have one or two rows of long tapering teeth, 10–20 cm long, set in a wooden head on a handle: wood, bone or (best) iron. Teeth 1 cm apart are about right.

  1. Fix one comb upright to a post or table. Lash on the wool by flicking its cut ends onto the teeth until they are half full.
  2. With the second comb, swing down through the tips of the fibre, a little deeper each stroke, until the fibre has moved onto the second comb. Then swap and comb back. Warming the combs (in hot water, or near the hearth, as the old wool-combers did) makes the work easier.
  3. Draw off the combed fibre by pulling it from the comb in a continuous ribbon, called top. The short fibres that stay behind on the comb (noils) go to carding or felt.

Top spun with the fibres lying parallel gives worsted yarn: smooth, hard-wearing, less fuzzy, ideal for warp threads, suits (Tailoring and Pattern Drafting) and stockings.

How to tell it worked

  • Clean wool feels dry and soft, not tacky, sticky or waxy; a handful squeezed and released springs back; it does not leave a greasy shine on your palm. It smells faintly of sheep, not of dung.
  • Not felted: the locks still pull apart easily and keep their crimp.
  • Good rolags are light, even, and you can see through them when held up to the light. Clumps and "neps" (little knots) mean the card was overloaded or the wool had second cuts.

Note Troubleshooting. Wool still sticky after washing → the water was too cool or cooled too long before lifting the wool out. Wash again hotter. Wool felted into mats → you stirred, squeezed hard, or moved it between hot and cold water. Matted wool can still become Felt or stuffing; it cannot be spun. Wool is yellow even when clean → that is its natural colour in some sheep, or old set grease. Sun-bleaching helps a little. Rolags full of lumps → overloaded cards, or short second cuts; tease more carefully first. Yarn breaks often → tender wool (it snapped in the flick test) or very short fibres. Use it for weft, not warp.

Dangers

Danger Anthrax ("wool-sorters' disease"). Fleeces and hides from animals that died of anthrax carry spores that can live for decades. Breathing the dust from sorting such wool causes a lung infection that is usually fatal. Never take wool, hair or skin from an animal that died suddenly of unknown cause, especially with dark blood oozing from the nose or mouth — bury or burn the carcass whole, without opening it. Sort and open dry wool outdoors or in a draught, and do not shake dusty fleece near your face.

  • Other diseases from sheep. Orf (scabby sores on lips and udders of sheep) and ringworm spread to hands. Wash after handling sheep and cover cuts. See Animal Health.
  • Cutting the sheep. Nicks are common at first. Clean cuts with clean water, and keep flies off: in summer, flies lay eggs in wounds and dirty wool ("fly-strike"), and maggots can eat a sheep alive within days. Check sheep often.
  • Overheating and chill. Shear sheep in cool weather, not in the midday heat. Give newly shorn sheep shelter for a few weeks.
  • Back injury. Shearing is back-breaking. Take breaks; lift sheep with your legs, not your back.
  • Hot water and stale urine. Scald risk with large tubs — lift wool out with sticks. Work with stale urine outdoors; the ammonia stings eyes.
  • Moths and beetles. Clothes moth and carpet beetle larvae eat wool. Store it clean and dry, in tight baskets or bags with cedar shavings, lavender, or tansy, and shake and sun it every few months.

What this unlocks

Spin it into yarn (Spinning and Weaving Cloth, The Spinning Wheel) and weave it (The Loom); knit it (Knitting, Crochet and Netting); or skip spinning and full it straight into Felt for boots, hats, blankets and yurts. Woollen cloth gives warm Making Clothes and socks for Footwear. Lanolin goes into ointments (Making Medicines) and leather care (Hides and Leather). Felted wool lines bellows and seals; woollen blankets and clothes make survival possible in Surviving Cold and Heat. Large-scale carding and combing are among the first jobs taken over by Textile Machinery.

How it was first done

Sheep were domesticated about 10,500–11,000 years ago in the hills of south-eastern Turkey and western Iran — at first for meat, milk and hides, since wild sheep are hairy, not woolly. Woolly sheep were bred slowly over the following millennia; by about 5,000–6,000 years ago, in Mesopotamia, wool was being gathered on a large scale, and clay tablets from Sumerian cities record flocks, wool rations and weaving workshops. For most of that time wool was plucked or combed out at the spring moult. Iron spring shears appeared in Europe and the Near East during the first millennium BC. Hand cards with wire teeth came into use in Europe in the Middle Ages, and wool combs are much older. Wool made medieval England rich — to this day the presiding officer of the House of Lords sits on a sack of wool, the Woolsack — and sheep remain the source of most of the world's wool.

Source: content/entries/textiles/wool.md