◆ Rebuild

Part 3 · Metals

Powder Metallurgy

Make metal as a fine powder, press it in a steel die and heat it in a protective gas until the grains weld together without melting. This gives oil-filled bronze bearings that never need greasing, iron gears that need no machining, metal filters, and parts of metals that cannot be melted at all.

Difficulty
●●●●●
Time
Weeks to make powders, a die and a furnace; then a few minutes to press a part and an hour or two to sinter a batch
Steps from zero
32 prerequisites →

You need first

Tungsten and Filament WireBearings and Lubrication

This unlocks

—
The full path from nothing — 32 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Salt
  13. Lime
  14. Fermentation
  15. Lye and Potash
  16. The Wheel and Axle
  17. Glass
  18. Bellows
  19. The Lathe
  20. Copper Smelting
  21. Iron (the Bloomery)
  22. Laboratory Glassware
  23. Blacksmithing
  24. Bronze
  25. The Battery
  26. Steel
  27. Bearings and Lubrication
  28. Electrolysis
  29. Copper Wire
  30. Iron and Brass Wire
  31. Hydrogen, Oxygen and Gases
  32. Tungsten and Filament Wire
  33. Powder Metallurgy

Do them roughly in this order. See it on the tech tree →

Why it matters

Casting pours molten metal into a mould; machining cuts a part out of a solid block. Powder metallurgy does neither. You press fine metal powder into the exact shape in a hardened steel die, then heat it until the grains weld to each other — sintering — without ever melting it. It gives you four things nothing else does:

  • Metals you cannot melt. Tungsten and tungsten carbide are made only this way (Tungsten and Filament Wire).
  • Holes on purpose. A pressed bronze bush can be one-quarter empty space, and those tiny pores hold oil. Such a self-oiling bearing runs for years in a fan, a sewing machine or a motor without ever being greased (Bearings and Lubrication). The same porous metal makes filters for fuel, oil, air and gas.
  • Mixtures that will not alloy. Copper with graphite for motor brushes (The Electric Motor), copper with tungsten for welding electrodes and switch contacts, iron with copper and carbon, all pressed together as powders.
  • Finished parts in one stroke. A small gear, cam or lever comes out of the press to size, with holes and teeth, no swarf and almost no waste. For parts needed by the thousand, it is cheaper than machining.

It leads on to cemented carbide tools (Tungsten and Filament Wire, Machine Tools), powder-iron cores for radios (Transformer Steel, Ferrite and Magnetic Shielding), sintered and ferrite magnets (Permanent Magnets), and the ceramic parts of Piezoelectric Crystals and Ceramics and spark plugs.

How it works

Sintering. Put two clean grains of metal in contact and heat them to roughly two-thirds to four-fifths of their melting point (measured from absolute zero). Their atoms start to wander. They move into the contact point and build a neck between the grains. The necks grow, the pores between grains shrink and round off, and the loose heap becomes one solid, if still porous, piece. Copper sinters well at 800–900 °C (it melts at 1,085 °C); iron at 1,100–1,150 °C (it melts at 1,538 °C).

Clean surfaces only. An oxide skin stops the atoms crossing. Fine powder has an enormous surface, and it rusts or tarnishes at once in hot air. So sintering is always done in a protective atmosphere: hydrogen, a gas rich in carbon monoxide made from charcoal, or packed in charcoal powder. These gases also strip off thin oxide already on the powder.

Liquid-phase sintering. If one powder melts at the sintering heat, it runs through the pores and speeds everything up. Tin (melts at 232 °C) mixed with copper powder melts, soaks into the copper grains and turns them into bronze. Cobalt does the same for tungsten carbide.

Pressing. Loose powder has about a third of the density of solid metal. Pressed hard in a die, the grains deform and lock together into a green compact — a part that holds its shape and can be handled gently, like hard chalk. Powder does not flow like a liquid: it rubs on the die wall. A tall part pressed from one end comes out dense at that end and loose at the other. That is why pressed parts are short and squat, and why good dies press from both ends.

Density decides everything. Iron is 7.87 g/cm³ solid. A self-oiling iron bearing is pressed to about 5.8–6.2; a gear to 6.6–7.0. The denser the part, the stronger, but the harder to press.

1 Fill Fill shoe Powder 2.5–3 × part Die Lower punch Core rod 2 Press 2–7 t/cm² Upper punch Green compact pressed from both ends 3 Eject Bush lift off lower punch pushes it out
Fig. 1 The pressing cycle. Powder fills the die from a shoe; the punches squeeze it from both ends; the lower punch pushes the green compact out. A core rod forms the hole of a bush.

What you need

Item Notes See
Iron oxide: hammer scale, mill scale or pure ore concentrate For iron powder Finding and Identifying Ores, Blacksmithing
Copper and tin For bronze powder Copper Smelting, Tin and Pewter
Hydrogen, or a charcoal gas producer Reducing and sintering atmosphere Hydrogen, Oxygen and Gases, Tungsten and Filament Wire
Graphite powder 0.5–1% in iron parts; die lubricant Pencils and Chalk
Stearic acid, wax or zinc stearate Pressing lubricant, 0.5–1% Soap
Sieves of fine brass or silk gauze To grade powder Iron and Brass Wire
Die of hardened tool steel, with punches One for each part Alloy and Stainless Steels, Presses, Punches and Dies
Press of 5–100 tonnes Screw, toggle or hydraulic Hydraulic Presses and Rams, Presses, Punches and Dies
Tube or muffle furnace to 1,150 °C With gas-tight retort Electric Kilns and Furnaces, The Kiln
Light machine oil To fill bearings Oils and Pressing, Petroleum and Refining

Where to find it

All the raw metals come from earlier chapters. The best starting point for iron powder is blacksmith's hammer scale — the black flakes that fall off red-hot iron around the anvil. It is nearly pure iron oxide with no sand or rock. Sweep it up, wash it, and keep it dry. Rich magnetite or hematite concentrate, crushed and separated with a magnet (Finding and Identifying Ores), also works, but every bit of sand left in it stays in the powder as hard grit. Graphite comes from natural flake graphite or from Lampblack and Carbon Black.

Making the powders

Powder size is given by the sieve it passes. A sieve with 100 wires to the inch (100 mesh) has holes of 0.15 mm; 200 mesh, 0.075 mm; 325 mesh, 0.045 mm. Most pressing powders pass 100 mesh, with not more than a quarter finer than 325 mesh. Filter powders are sieved to a narrow band, for example between 60 and 100 mesh.

Iron powder by reduction

  1. Grind dry hammer scale in a ball mill or under an edge-runner to pass 100 mesh (Portland Cement describes the mills).
  2. Reduce. Spread it 1–2 cm deep in iron trays and push them into a tube furnace with flowing hydrogen at 800–1,000 °C for 1–2 hours, exactly as for tungsten (Tungsten and Filament Wire). Water vapour streams out of the exit; when the exit gas no longer fogs a cold glass, it is done. Cool in hydrogen.
  3. Or reduce with charcoal. Pack alternate layers of scale and fine charcoal (about 1 part charcoal to 3 of scale by weight), with a little limestone powder to take up sulfur, in fireclay pots (saggers) with lids luted on with clay. Heat them in a kiln at about 1,100–1,200 °C for 1–2 days (The Kiln). The oxide becomes a cake of spongy iron. Crush it, sieve it, and anneal it in hydrogen at 800–900 °C to burn out leftover carbon and soften the grains. This sponge iron is the classic pressing powder: its rough, porous grains lock together well.
  4. Store it in sealed tins. It rusts quickly in damp air.

Copper powder by electrolysis

Electrolytic copper powder is very pure and presses beautifully.

  1. Make a bath of 15–30 g of copper per litre (as copper sulfate, Sulfuric Acid) with 150–200 g of sulfuric acid per litre — much less copper and more acid than a plating bath (Electroplating).
  2. Hang copper anodes and smooth copper or lead cathodes, and run at 10–30 A per dm² of cathode, ten times plating density, at 40–50 °C.
  3. The copper grows on the cathode as a loose, dark, fern-like sponge instead of a smooth coat. Every 15–30 minutes, brush it off into the bottom of the tank.
  4. Collect it, wash it free of acid with many changes of water, then rinse in water with a little soap or gelatin to slow tarnishing. Dry it quickly at under 100 °C.
  5. Anneal it in hydrogen at 400–500 °C for 30 minutes to remove oxide and soften it. Crush the lightly caked lumps gently and sieve.

Atomised powders

Molten metal poured as a thin stream through a strong jet of water, steam or air breaks into droplets that freeze as powder. Tin is easy: melt it, pour a pencil-thin stream onto a fast-turning wet iron disc or into a jet from a pump, and collect it under water. Bronze filter powder needs round grains: pour molten bronze (90 copper, 10 tin) through a 3–5 mm hole in a clay crucible bottom into a fan-shaped jet of water or steam, or let it drip from 3–4 m into a tall tank of water. Sieve the result and keep only the round fraction you want.

Filings and grinding

Brittle metals (bismuth, antimony, cast iron, ferro-alloys) can be ground in a ball mill. File dust of iron or brass works for experiments, but it is oily and coated in oxide: wash it in spirit and reduce it in hydrogen first.

The compacting die

  1. Die. A thick-walled ring of hardened tool steel — high-carbon or chromium steel (Alloy and Stainless Steels) — whose bore is the outline of the part. Wall thickness at least equal to the bore diameter. Harden to file-hard and temper only to straw. Lap the bore mirror-smooth; any scratch tears every part. Give the top 3–5 mm a slight flare so powder enters, and give the bore no taper at all, or a few hundredths of a millimetre wider at the exit end so the part does not crack as it springs out.
  2. Punches. An upper and a lower punch, a sliding fit in the bore with 0.01–0.03 mm clearance. Too loose and powder squeezes into the gap.
  3. Core rod. For a bush, a polished hardened rod running up through the lower punch forms the hole.
  4. Fill depth. Loose powder is about 2.5–3 times as tall as the finished part. A bush 10 mm long needs a die cavity at least 25–30 mm deep when the lower punch is down.
  5. Pressing from both ends. Either let the die body float on springs, so it moves down as the upper punch presses and the lower punch effectively presses too, or push both punches at once. Keep parts no taller than about twice their diameter.

Force needed. Pressure × area. A bronze bush 16 mm outside and 10 mm inside has an end area of 1.2 cm². At 3 tonnes per cm² it needs about 3.7 tonnes — a hand screw press or a small hydraulic jack. An iron gear 30 mm across with a 10 mm hole (6.3 cm²) at 6 tonnes per cm² needs nearly 40 tonnes. Make sure your press, and your die, can take it.

Part Powder Pressure Green density
Self-oiling bronze bush 90 Cu + 10 Sn, 0.5–1% graphite 2–3.5 t/cm² 6.0–6.6 g/cm³
Self-oiling iron bush Iron, 1–2% copper, 0.5% graphite 3–4 t/cm² 5.8–6.2 g/cm³
Iron gear or cam Iron, 2% copper, 0.6–0.8% graphite 5–7 t/cm² 6.6–7.0 g/cm³
Bronze filter Round bronze grains, sieved None (loose) about 5 g/cm³

Step by step: a self-oiling bronze bearing

Housing cast iron or steel Sintered bronze bush a quarter of it is oil-filled pores Oil film seeps out when warm Turning shaft Pores full of oil Grains joined by necks Seen magnified grains 0.05–0.15 mm
Fig. 2 A self-oiling bearing. The sintered bronze is about a quarter pores, filled with oil. When the shaft turns and warms, oil seeps out to make a film; when it stops and cools, the pores draw the oil back in.
  1. Mix. 90 parts copper powder, 10 parts tin powder, 0.5–1 part fine graphite, 0.5–1 part powdered stearic acid or wax as lubricant. Tumble in a closed jar for 30 minutes. Do not grind it — just mix.
  2. Lubricate the die. Brush the bore and core rod with a thin paste of graphite or stearic acid in spirit.
  3. Fill. Lower punch down, scrape the powder level with the top of the die with a straightedge. Every fill must be the same, or parts come out different lengths.
  4. Press. Press steadily, not with a blow, to the set stop (a collar on the upper punch, or a mark) — about 3 tonnes per cm². Hold for a second.
  5. Eject. Lift the upper punch and push the lower punch up until the green bush stands free. Lift it off with fingers. It should be smooth, with sharp edges, and should not crack when you squeeze it gently.
  6. Burn off the lubricant. Heat the green parts slowly to 400–500 °C in the protective atmosphere, or in a loosely closed box, and hold 20–30 minutes so the wax leaves as vapour before the part closes up. Rush this and the parts blister.
  7. Sinter at 780–830 °C for 15–30 minutes in hydrogen or charcoal gas. The tin melts and soaks into the copper. The bush grows very slightly. Cool in the same atmosphere until below 150 °C, or it comes out black.
  8. Size. Press each bush once more through a polished sizing die with a sizing core rod, to bring the bore and outside to exact size (within about 0.01–0.02 mm) and smooth the bore.
  9. Fill with oil. Drop the bushes into light machine oil at 80–100 °C for 1–2 hours, then let them cool in the oil overnight. The cooling oil is pulled into the pores. Better: put them in oil in a closed jar, pump the air out (The Vacuum Pump), then let the air back in. A good bush takes up oil equal to 18–25% of its volume.
  10. Fit. Press the bush into its housing with a smooth plug, which closes the bore slightly; allow for it. Leave 0.02–0.04 mm running clearance on a 10 mm shaft.

Sintered iron gears

  1. Mix iron powder with 2% copper powder, 0.6–0.8% graphite and 0.75% lubricant.
  2. Die. The die bore is the gear outline, teeth and all, cut by careful filing and grinding into a split die, or by spark or wire cutting when you have it. The punches carry the same tooth outline. This die is expensive and only pays for runs of thousands (Gears).
  3. Press at 5–7 t/cm², pressing from both ends.
  4. Delube at 400–600 °C, then sinter at 1,120 °C for 20–30 minutes in hydrogen or in a carbon-monoxide-rich gas made by passing a little air over glowing charcoal. The graphite dissolves into the iron and makes it a mild to medium steel; the copper melts and strengthens it. The part shrinks or grows by a few tenths of a percent — measure the first batch and adjust the die.
  5. Finish. Size for accuracy. For wear, harden like steel (Steel), or treat it in steam at about 550 °C for an hour: the pores fill with hard black iron oxide, which seals them and resists wear.

Do not press side holes, undercuts, threads or grooves running round the part — they cannot come out of a straight die. Keep walls at least 1.5–2 mm thick, round all corners slightly, and avoid thin feather edges on the punches.

Sintered filters

  1. Sieve round bronze grains to a narrow size range: for example 0.15–0.25 mm for a coarse fuel filter, 0.05–0.10 mm for fine work. The pores are roughly a fifth of the grain size.
  2. Pour the loose grains into a mould of graphite, fireclay or steel coated with graphite, the shape of the filter: a disc, a cup or a tube. Tap it to settle them. Do not press.
  3. Sinter at 850–900 °C for 30–60 minutes in a reducing atmosphere. The grains weld only at their contact points.
  4. Clean in hot water and spirit, and blow dry.

A filter of nickel or stainless powder resists acids better; iron filters are cheap but rust.

Simple sintering furnaces

  • Tube furnace with hydrogen, as built for Tungsten and Filament Wire — the best.
  • Pack sintering. Lay the parts on a bed of alumina or fine sand in a steel box, cover them, and lay a layer of charcoal powder on top under a lid sealed with clay. Heat the whole box in a muffle furnace or forge. The charcoal makes carbon monoxide that protects the parts. It works for bronze and iron; iron parts pick up some carbon.
  • Gas producer. Blow a small, steady stream of air up through a tall pipe of glowing charcoal: the gas coming out is about one-third carbon monoxide, the rest nitrogen. Pass it through the furnace retort and burn it at the exit.

Hard metal tips

Cemented carbide — tungsten carbide grains bonded with cobalt, liquid-phase sintered at 1,400–1,500 °C — is covered fully in Tungsten and Filament Wire.

When it beats casting and machining

Use powder metallurgy when Use casting or machining when
Thousands of identical small parts, under about 1 kg A few parts, or large ones
The metal cannot be melted (tungsten, carbide) Full strength and toughness matter most
You want pores: bearings, filters The part needs undercuts, threads, side holes
You want mixtures: copper–graphite brushes, copper–tungsten contacts The die would cost more than the parts
Little waste matters (95% of the powder ends in the part) The part is tall and thin

How to tell it worked

  • Density. Weigh a sintered part in air, then seal it by dipping in melted wax and weigh it hanging in water (Measurement from Scratch). Weight in air divided by the loss of weight in water gives its density. Compare with the target in the table.
  • Fracture. Break a test part. The break should be grey, granular and even right through, with no layers or cracks parallel to the ends.
  • Ring. A well-sintered part rings when dropped on stone; a poorly sintered one clicks dully.
  • Oil. Warm an oiled bearing in your hand or on a warm stove: tiny beads of oil sweat out all over the surface. Wipe it and they come back.
  • Filter. Wet a filter with spirit, hold it under water and blow gently through it. The first bubbles should come evenly from the whole surface at a low pressure; a stream from one spot means a crack or a large pore.

Note Troubleshooting. Green part cracks across on ejection → too much pressure, a die bore that narrows at the exit, or too little lubricant. Lap the exit slightly wider and lubricate. Part dense at one end, crumbly at the other → pressed from one end only, or part too tall. Press from both ends. Part blistered or swollen after sintering → lubricant burned off too fast. Hold longer at 400–500 °C first. Part soft, crumbly and dark after sintering → the atmosphere let air in, or too cool. Check the retort for leaks; sinter hotter or longer. Bronze part grew too much, or has tin sweat on it → tin powder too coarse or heated too fast. Use finer tin and a slower heat-up. Parts different lengths → uneven fill. Level every fill the same way.

Dangers

Danger Hydrogen and carbon monoxide. Hydrogen mixed with air explodes; flush every retort with gas until the exit gas burns quietly before heating, and burn all exit gas. Carbon monoxide from charcoal gas and pack sintering kills without warning — work outdoors or under a strong draught, and burn the exit gas. See Tungsten and Filament Wire and Hydrogen, Oxygen and Gases.

Danger Burning and exploding dust. Very fine iron, aluminium and magnesium powders, and freshly reduced powders of any metal, can catch fire by themselves in air, and a cloud of fine metal dust can explode like flour dust. Cool reduced powder fully in the protective gas, let air in slowly, keep powders in closed tins, never sieve fine powder near a flame or spark, and sweep rather than blow up dust.

  • Breathing dust. Wear a damp cloth mask when sieving. Nickel and cobalt powders harm lungs and skin; never breathe them.
  • Dies under load. A cracking die at 40 tonnes throws steel fragments. Guard the press and stand to one side.
  • Electrolytic baths are acid: see Electroplating.

Going further

Pressing and sintering, then pressing again and sintering again, gives near-solid parts. Forging a hot sintered blank once in a closed die (Anvils, Trip Hammers and Power Hammers) makes connecting rods as strong as wrought steel. Powder iron mixed with resin makes the cores of radio coils (Transformer Steel, Ferrite and Magnetic Shielding); alnico and ferrite magnets are pressed and sintered too (Permanent Magnets). Pressing powder into a cold die with a little wax and then sintering is also how alumina spark-plug insulators and many ceramics are shaped (Stoneware and Porcelain).

How it was first done

Metalworkers on the Pacific coast of what is now Ecuador and Colombia, some 2,000 years ago, heated grains of platinum with gold dust and hammered them into small ornaments — a kind of sintering — long before Europeans could work platinum at all. In the early 1800s William Hyde Wollaston in London made workable platinum by pressing purified platinum powder, heating it and forging it, publishing his method in 1829 (Platinum and the Platinum Metals). In 1909–1910 William Coolidge at General Electric made ductile tungsten wire from pressed and sintered powder (Tungsten and Filament Wire). German workers developed cemented carbide in the early 1920s, sold by Krupp from 1926 as Widia. Porous self-oiling bronze bearings were developed in the 1920s and 1930s, notably by American car makers — Chrysler's Oilite name is still used — and sintered iron machine parts spread in large numbers after the Second World War. In Sweden, the Höganäs works began making sponge iron by reducing ore with coke in saggers around 1910, and became the world's great source of iron powder.

Source: content/entries/metals/powder-metallurgy.md