◆ Rebuild

Part 15 · Knowledge and Science

Wood Pulp, Kraft Paper and Paperboard

Rags run out long before the need for paper does. Grinding logs on a stone, or cooking wood chips in lye, sulfite or sulfide liquor, frees the fibres of any forest. Machines that form paper continuously on a moving wire or a turning cylinder then make it by the kilometre, as newsprint, tough brown kraft paper, and the board that boxes the world's goods.

Difficulty
●●●●●
Time
A hand-cooked batch of soda pulp in a day; a small cylinder machine is a season's work; a pulp mill is an industry
Steps from zero
6 prerequisites →

You need first

PaperLye and PotashSulfur

This unlocks

—
The full path from nothing — 6 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Sulfur
  4. Pottery
  5. Lye and Potash
  6. Paper
  7. Wood Pulp, Kraft Paper and Paperboard

Do them roughly in this order. See it on the tech tree →

Why it matters

Hand papermaking (Paper) needs rags, hemp, flax or bark, and by the early 1800s Europe and America were so short of rags that papermakers advertised for old linen door to door. Wood solved it: a forest, cut and replanted in turn (Forestry and Tree Nurseries), is a near-endless store of fibre. Two inventions together made paper cheap enough for daily newspapers, schoolbooks, bags, labels and cardboard boxes. Pulping turns logs into fibre by grinding or cooking, and the paper machine forms paper continuously, more in an hour than a hand mill made in a year. This chapter covers both, and the kraft paper, paperboard and packing materials they make possible.

How it works

Dry wood is roughly:

Part Share What it is
Cellulose 40–50% Long chain molecules bundled into fibres. This is what you want.
Hemicelluloses 25–35% Shorter sugar chains. They help fibres bond, but dissolve in strong cooking.
Lignin 20–30% The brown "glue" that cements fibres together and stiffens the tree. It yellows in light and stops fibres bonding.

Softwood fibres (spruce, pine, fir) are 3–4 mm long and make strong paper. Hardwood fibres (birch, poplar, beech) are about 1 mm long and make smooth, opaque paper. Cotton and linen fibres are far longer, which is why rag paper is so strong.

There are two ways to free the fibres:

  • Mechanical pulping grinds the wood apart. 90–95% of it becomes pulp, lignin and all, but the fibres are short and broken, and the paper is weak and yellows in sunlight. Cheap: for newsprint and the middle of boards.
  • Chemical pulping cooks chips in a liquor that dissolves the lignin and leaves the fibres whole. Only 40–55% becomes pulp, but it is strong and lasting. The liquors are soda (caustic soda), sulfite (an acid from burnt sulfur and lime) and kraft (caustic soda with sodium sulfide).

What you need

For Needs
Groundwood Debarked logs of spruce, fir or poplar; a big sandstone grindstone; a lot of power: about 1,000–2,000 kWh per tonne of pulp (Water Turbines and Hydroelectric Power, The Waterwheel).
Soda pulp Caustic soda (Lye and Potash, Soda Ash and Baking Soda, Lime); wood chips, mostly hardwood; a steel pressure cooker (Pressure Vessels and Valves, Boilers and Pressure Vessels).
Sulfite pulp Sulfur to burn; limestone (Lime); an acid-proof digester lined with brick.
Kraft pulp Caustic soda plus sodium sulfide, made from sodium sulfate (salt cake, found as the mineral mirabilite, or made from salt and Sulfuric Acid) reduced in a furnace; a steel digester; a recovery furnace.
For all Plenty of clean water, about 50–100 m³ per tonne of paper even with reuse (Water Treatment for a Town); screens; a beater (Paper).

Debarking and chipping

  1. Cut spruce, fir, pine, poplar or birch into 1–1.2 m lengths.
  2. Debark it (bark makes dark specks): strip it with a drawknife or barking spud when the sap runs in spring, or tumble the logs with water in a rotating drum. Burn the bark.
  3. Chip it for chemical pulping, into chips 15–25 mm long along the grain and 3–5 mm thick. A chipper is a heavy iron disc 1–2 m across with three or four knives in slots across its face, spinning at a few hundred rpm, fed endwise down a spout at about 40°. Screen out dust and oversize: even chips cook evenly.

Method 1: Groundwood pulp

Groundwood grinder Digester and blow tank Press 1–2 bar Logs in pocket along the stone's axis 20–30 m/s Sandstone 1.2–1.8 m Water Pit: pulp and water to the screens Chips in Chips in liquor 160–175 °C 7–9 bar, steel shell steam in Blow valve steam Blow tank chips burst into fibre; to washing
Fig. 1 Two ways to free wood fibre. In the grinder, logs are pressed against a wet revolving sandstone that tears off fibres, and water carries the pulp away. In the digester, chips are cooked in liquor under steam pressure, then blown into a tank where they burst into fibre.

The pulp grinder is a grindstone that tears logs apart into fibres under water.

  1. The stone. Fine, even sandstone (Quarrying and Cutting Stone) 1.2–1.8 m across and 40–60 cm wide, on a strong shaft in heavy Bearings and Lubrication, driven directly by a water turbine at a surface speed of 20–30 m/s (250–380 rpm for a 1.5 m stone). Ring it with a hammer first: a cracked stone clunks (Precision Grinding).
  2. The pockets. Boxes against the stone face, each holding 3–6 logs parallel to the stone's axis, pressed on by a piston worked by weighted lever, screw or water pressure (Hydraulic Presses and Rams) at about 1–2 bar.
  3. Water sprayed on the stone below each pocket keeps the face at 60–80 °C so the fibres do not scorch; a pit below catches the pulp.
  4. Sharpening. Every few days roll a grooved hardened-steel burr across the face. A sharp stone makes coarse, fast pulp; a dull one, fine, slow pulp.
  5. Screen through slots 0.2–0.3 mm wide; splinters (shives) go back for regrinding. Thicken on a turning wire cylinder or in a sack.

Groundwood alone is too weak for a paper machine. Newsprint is about 75–85% groundwood and 15–25% chemical pulp. It takes ink well but yellows within a few years: keep records on rag or chemical paper (Libraries and Preserving Knowledge).

Method 2: Soda pulp

The soda process is the simplest chemical pulp. It uses only caustic soda, which this book has already made from soda ash and lime (Lye and Potash). It works best on hardwoods and straw.

A small hand batch:

  1. Fill a steel pressure cooker or a small digester (Pressure Vessels and Valves) with chips of poplar or birch, or with chopped straw.
  2. Add caustic soda at 15–20% of the dry weight of the wood, in about 4 litres of water per kg of wood.
  3. Close the vessel and heat it to 160–170 °C (about 6–7 bar of steam pressure) for 2–4 hours. Without a pressure vessel, straw and grass will pulp at a boil (100 °C) in 3–6 hours, but wood chips will not soften properly.
  4. The test: a cooked chip crushes between finger and thumb into a soft mush of fibres.
  5. Drain off the dark brown black liquor (save it), wash the pulp well with hot water on a cloth or screen, and beat it in a mortar or a Hollander beater (Paper).

The pulp is pale brown and makes good paper. Bleach it, if you need white paper, with hypochlorite (bleaching powder) in two or three stages with washing between (Chlorine and Bleach).

Method 3: Sulfite pulp

The sulfite process gives a pale, easily bleached pulp, ideal for fine writing and printing papers, and pure enough for making rayon (Rayon and Nylon). It works on spruce and fir, but not on resinous pines.

  1. Make the acid. Burn sulfur in a brick oven with a controlled draught (Sulfur). Cool the sulfur dioxide gas, and pass it up a tall tower packed with lumps of limestone, with water trickling down. The gas dissolves and attacks the limestone, giving calcium bisulfite in a liquor that also contains free sulfur dioxide.
  2. The digester. The acid corrodes plain steel. So the digester is a steel shell, lined with acid-proof brick set in a lead or silica-cement mortar.
  3. Cook spruce chips in the acid at 125–145 °C and 5–7 bar for 6–12 hours, raising the heat slowly over the first few hours. If you heat it too fast, the chips burn: they turn black and hard as the lignin cross-links before the acid can soak in.
  4. Blow, wash and screen as for kraft (below).

The problem: calcium sulfite liquor is not easily recovered. Early mills poured it into rivers and killed the fish for miles. Evaporate and burn it, ferment its sugars to alcohol (Fermentation), or keep the mill small.

Method 4: Kraft pulp

Kraft (German and Swedish for "strength") is the strongest pulp, and today makes most of the world's paper. It works on any wood, including pine. Its secret is a liquor that pulps fast without weakening the cellulose, and a cycle that recovers nearly all of its chemicals.

Digester cook chips Washers rinse liquor out Evaporators thicken to 60–70% solids Recovery furnace burn lignin, melt salts Dissolving tank smelt + water Causticiser add quicklime Lime kiln burn mud to lime Wood chips pulp + liquor black liquor Pulp to beater and paper machine thick black liquor Salt cake makes up losses steam smelt: soda + sulfide green liquor White liquor caustic soda + sodium sulfide mud lime fuel in, CO₂ out over 95% of the soda is reused
Fig. 2 The kraft cycle. White liquor cooks the chips; the spent black liquor is washed out, evaporated and burned in the recovery furnace, which makes steam and a smelt of soda and sodium sulfide; dissolved in water this gives green liquor; lime turns it back into white liquor; the lime mud is burned back to lime in a kiln.

The cook

  1. White liquor: caustic soda and sodium sulfide in water. About a quarter to a third of the active chemical is sulfide. Use about 16–20% active chemical on dry wood.
  2. Pack the chips into the digester and fill it with liquor, at about 4 parts liquor to 1 part wood.
  3. Steam it up to 160–175 °C (7–9 bar) over about an hour, and hold it there for 1–2 hours.
  4. Blow. Open a valve at the bottom of the digester and let the pressure blow the whole contents into a blow tank. The softened chips burst into fibre as the pressure drops. The steam is condensed for its heat.
  5. Wash the pulp on screens or vacuum drums with hot water, counter-current (cleanest water on the cleanest pulp), to recover as much black liquor as you can.

Unbleached kraft pulp is brown. It is used that way for sacks, wrapping and boxes. It can be bleached white, but it needs more bleaching than sulfite pulp.

The recovery cycle

  1. Evaporate the weak black liquor in a row of steam-heated pans or tube evaporators (the steam from each pan heats the next) until it is thick enough to burn: about 60–70% solids.
  2. Burn it in a recovery furnace. The dissolved lignin burns and raises steam for the mill (Boilers and Pressure Vessels). The sodium salts melt into a smelt at the bottom. Add salt cake (sodium sulfate) to make up losses. In the hot, carbon-rich bottom of the furnace, it is reduced to sodium sulfide, which is why kraft is also called the sulfate process.
  3. Dissolve the smelt in water to make green liquor (sodium carbonate and sodium sulfide).
  4. Causticise: add quicklime (Lime). It turns the carbonate back into caustic soda, giving white liquor, and settles out as lime mud (calcium carbonate).
  5. Reburn the lime mud in a lime kiln to quicklime, and use it again.

A good mill recovers over 95% of its sodium. Without recovery, kraft would be ruinously costly and would poison the river.

Beating and refining

Pulp from any process must be beaten before it makes good paper (Paper). The Hollander beater is an oval tub with a bladed roll running over a bladed bedplate. It brushes and frays the fibres, so they bond into a strong sheet. For mills, the Jordan refiner is a bladed cone turning inside a bladed shell, through which pulp is pumped continuously. Beat lightly for absorbent paper and board, and heavily for strong, dense, crisp paper.

The paper machine

The Fourdrinier machine

Headbox Endless wire shaken side to side Couch roll Press rolls Felt Steam-heated dryers 100–130 °C Calender Reel table rolls suction boxes water drains away direction of travel 99% about 80% 55–65% 5–8% water left in the web at each stage
Fig. 3 The Fourdrinier paper machine. Thin pulp flows from the headbox onto a moving endless wire; water drains through it, helped by table rolls and suction boxes; the couch roll lifts the wet web off onto a felt; press rolls squeeze out more water; heated cylinders dry it; the calender polishes it; and it is wound on a reel. Figures show how much of the web is still water at each stage.

The paper machine does on a moving belt what the vatman and coucher do by hand:

  1. Stock. Beaten pulp diluted to 0.5–1% fibre, with size and fillers (rosin, alum, clay) added (Paper).
  2. Headbox. Releases the stock evenly across the width through an adjustable slot, the slice, onto the wire at about wire speed.
  3. Wire. An endless belt of bronze wire cloth, 25–30 wires per cm (Iron and Brass Wire), running over a table of small rolls. Water drains through; early machines shake the wire sideways so the fibres cross, and suction boxes further on pull more water. A dandy roll can press in a watermark.
  4. Couch roll. At the end of the wire the web, about 20% fibre, is pressed onto a woollen felt (Felt) and lifted off.
  5. Presses. Two or three pairs of heavy rolls squeeze it to 35–45% fibre.
  6. Dryers. Cast-iron cylinders 1–1.8 m across, steam-heated to 100–130 °C (Boilers and Pressure Vessels), with felts holding the web on, dry it to 92–95%.
  7. Calender (a stack of polished chilled-iron rolls, The Blast Furnace and Cast Iron) smooths it, and it winds onto a reel.

Running it. Each section turns slightly faster than the one before (the draw) to keep the web taut, set on early machines by line shaft and cone pulleys (Belts, Chains and Power Transmission). Machines of about 1810 were 1–1.5 m wide and made 5–10 m a minute; modern ones run at over 1,500 m a minute.

The cylinder machine

The cylinder machine (or vat machine) is easier to build than the Fourdrinier, and is the natural machine for board. Build it first.

Couch roll presses felt on the cylinder Woollen felt moves left to right Press rolls plies knit together 1 ply 2 plies 3 plies Board to the dryers Vat of thin stock 0.3–0.5% fibre Wire-covered cylinder water drains inward and out of the open end; fibre stays on the wire each vat adds a ply
Fig. 4 The cylinder board machine. In each vat a wire-covered cylinder turns in thin pulp; water drains inside it, leaving a layer of fibre on its surface. A felt running over all the vats picks up each layer in turn, building up a thick board, which goes to the press and dryers.
  1. The vat. A wooden or concrete tank, a little wider than the paper, filled with stock at about 0.3–0.5% fibre and kept stirred.
  2. The cylinder. A hollow drum 60–120 cm across, made of brass or bronze rods or a spiral of wire over spokes, covered with a coarse backing wire and then a fine face wire (25–30 wires per cm). It turns slowly in the vat, about two-thirds under the stock. One end opens to a channel kept 10–30 cm lower than the stock level, so water flows inward through the wire and drains away. The fibres stay on the outside as a thin web.
  3. The couch. A woollen felt runs over the top of the cylinder, pressed lightly against it by a felt-covered couch roll. The wet web sticks to the felt and leaves the wire.
  4. Press and dry as for the Fourdrinier, or, for a small mill, cut the wet board from the felt into sheets and dry them in a warm, airy loft on racks.

Making board. Set 2–8 vats in a row under the same felt. Each cylinder adds a layer, or ply, on top of the last while they are all still wet, and the plies knit together in the press. Use cheap pulp (groundwood, waste paper, straw) for the inside plies and a clean, strong pulp for the outside plies.

A small cylinder machine 40–60 cm wide, turning at a few metres a minute, can be driven by a water wheel and make a few hundred kilograms of board a day.

The papers and boards

Kraft paper

Kraft paper is made from unbleached kraft pulp, beaten only moderately, so that it keeps long, strong fibres. It is brown, tough, and hard to tear.

Grade Weight Use
Wrapping kraft 40–80 g/m² Parcels, paper bags (Sacks, Boxes, Crates and Packaging)
Sack kraft 70–100 g/m² Multi-wall sacks for cement, flour, fertiliser: 3–5 plies, glued or sewn
Kraft liner 125–300 g/m² The outside faces of corrugated board
Gummed tape 60–90 g/m² Coated with animal glue or starch, wetted to stick

Good kraft paper is even, with no thin spots when held up to the light, and resists a strong pull. A strip 15 mm wide of 80 g/m² sack kraft should hold about 8–10 kg hanging from it. Torn, its edge shows long fibres sticking out like hairs.

Paperboard

Paperboard is any paper thicker than about 0.3 mm, or heavier than about 200–250 g/m². The main kinds are:

  • Greyboard (chipboard): repulped waste paper, soaked a day, beaten, screened and formed on a cylinder machine or couched thick by hand (Sacks, Boxes, Crates and Packaging). For book covers (Bookbinding) and partitions.
  • Strawboard: straw cooked 6–10 hours with 10–15% lime on its weight, beaten and formed. Yellow and stiff.
  • Folding boxboard, 0.3–0.6 mm: a white chemical-pulp top ply to print on, a bulky groundwood middle and a clean back. For cartons.
  • Linerboard (kraft) for the faces of corrugated board, and corrugating medium (part-cooked hardwood pulp) for its flutes.
  • Solid board: plies laminated to 1.5–3 mm for heavy cases (Bags, Backpacks, Wallets and Luggage).

Testing board. Fold it sharply both ways along a crease. Good board folds cleanly without cracking along the crease. Then press a ruler edge onto a strip held flat and see how much load it carries before it buckles: stiffness matters more than strength in a box.

Wood wool and other packing

Wood wool (excelsior) is long, curly, straw-fine wood shavings: springy, cheap and clean, for packing glass, pottery and fruit, stuffing upholstery (Mattresses and Upholstery), evaporative cooler pads (Ice and Refrigeration) and boards.

Making it.

  1. Use seasoned, knot-free logs of poplar, aspen, lime, pine or spruce, about 50 cm long.
  2. By hand: clamp the log on a bench and draw a sharp plane across its side. The plane's iron should be set to cut 0.1–0.4 mm deep. Fix a row of small, sharp spurs in front of it, 2–5 mm apart, which score the wood so that the shaving comes away in narrow strands.
  3. By machine: the log is pressed against a bed, and a carriage carrying the spurs and a long knife slides back and forth across it, driven by a crank at 60–120 strokes a minute (Cranks, Cams and Linkages). A weight or spring advances the log after each cut. One machine makes roughly 50–150 kg of wood wool an hour.
  4. Grades range from "superfine" (0.1 mm, for delicate packing) to coarse (0.5 mm and 5 mm wide, for boards and stuffing). Bale it under a press.

Wood wool board

Wood wool board is wood wool bonded with cement into light, stiff slabs for walls, ceilings, roof decks and sound-deadening panels (Insulation and Keeping Buildings Warm or Cool).

  1. Soak coarse wood wool in water containing about 2–3% calcium chloride or water glass (Water Glass (Sodium Silicate)). This stops the wood's sugars from spoiling the cement set.
  2. Toss the damp wool in Portland cement (Portland Cement), about 2 parts cement to 1 part wood wool by weight, until every strand is coated.
  3. Spread it loosely in a mould to the thickness wanted, 25–75 mm, and press it lightly.
  4. Leave it for a day, then unmould it and cure it damp for two weeks.

The board weighs 350–600 kg/m³. It can be sawn and nailed, and plastered directly. It resists fire and rot, and termites leave it alone.

Other packing. Shredded waste paper, crumpled kraft, moulded pulp trays and cups (Sacks, Boxes, Crates and Packaging), sawdust, cork crumbs, dry moss and straw all do the same job: they hold an object still and soften blows.

How to tell it worked

  • Pulp: a pinch shaken in a jar of water spreads into separate fibres with no lumps or splinters.
  • Machine paper: even against the light, with no holes or thin streaks; it tears straighter along the machine direction than across it.
  • Board: the plies do not split when bent hard or soaked for an hour.

Note Troubleshooting. Groundwood full of splinters → stone dull, unevenly burred, or pressure too high. Re-burr, ease the load. Chips uncooked in the middle → chips too thick, liquor too weak, or heating too fast. Chip thinner and cook longer. Sulfite chips black and hard → "burnt" cook from heating too fast. Raise the heat slowly over 3–4 hours. Paper lumpy and cloudy against the light → stock too thick, or headbox flow uneven. Dilute, and even out the slice. Web breaks between sections → draw too large or web too wet at the couch. Ease the speed difference, and improve drainage and suction. Paper cockles (wavy) as it dries → uneven drying. Hold it tight against the dryers with felts. Board plies split → plies too dry when joined, or press too light. Join them wetter and press harder.

Dangers

Danger Digesters can explode. A digester is a large vessel of boiling caustic or acid liquor under 6–9 bar. Build it as a proper pressure vessel, test it with water at 1.5–2 times working pressure, fit a safety valve, and never open it or work its lid before the pressure gauge reads zero (Pressure Vessels and Valves, Boilers and Pressure Vessels). A blow valve opened by accident can spray scalding pulp across the room.

Danger Deadly gases. Kraft and black liquor give off hydrogen sulfide (rotten-egg smell). In strong doses it deadens the sense of smell and kills in minutes, and it collects in tanks, pits and drains. Sulfite mills breathe out sulfur dioxide, which chokes, and bleaching gives off chlorine. Never enter a tank or pit without blowing air through it first, a rope on your waist, and a second person outside (Mining and Tunnelling).

  • Caustic liquor blinds and burns: eye protection, gloves, and lots of water at once (Acids, Bases and Testing).
  • Roll nips pull in hands and arms in an instant. Guard every nip; stop the machine before threading a broken web.
  • Grindstones can burst: check for cracks and never overspeed.
  • Fire. Dry paper, dust and wood wool burn fast (Firefighting).
  • Rivers. Recover chemicals, settle out fibre and treat the rest (Water Treatment for a Town).

What this unlocks

Cheap wood-pulp paper is what makes daily newspapers, cheap books and Libraries and Preserving Knowledge, mail, office paper and school exercise books possible. Kraft and board make the bags, sacks, boxes and cartons of all trade (Sacks, Boxes, Crates and Packaging). Pure cellulose from sulfite and kraft pulp is the raw material for rayon and cellophane (Rayon and Nylon, Early Plastics), nitrocellulose for film (Photography), and filter papers (Burners, Stands and Laboratory Equipment). The steam and power plant of a pulp mill burns its own bark and lignin, and its waste heat can heat a town (Heat Pumps and District Heating).

How it was first done

René Réaumur suggested in 1719 that paper could be made from wood, as wasps make their nests. Jacob Christian Schäffer made test papers from wood and many plants in the 1760s, and Matthias Koops in London printed a book on straw and wood paper in 1800. Louis-Nicolas Robert built the first continuous paper machine in France in 1798–1799. Henry and Sealy Fourdrinier financed its development in England with the engineer Bryan Donkin, and their improved machine was working by 1803–1807. John Dickinson patented the cylinder machine in 1809.

Friedrich Gottlob Keller, a Saxon weaver, made paper from ground wood around 1843–1844, and Heinrich Voelter turned it into an industry. Charles Fenerty in Nova Scotia did similar experiments at about the same time. Hugh Burgess and Charles Watt developed the soda process in the 1850s. The American chemist Benjamin Tilghman patented the sulfite process in 1866–1867, and the Swede Carl Daniel Ekman ran the first successful sulfite mill in the 1870s. Carl F. Dahl invented the kraft process in Danzig in the early 1880s, and the first kraft mill opened in Sweden in 1890. Kraft took over the world only after G. H. Tomlinson's recovery furnace of the 1930s made chemical recovery cheap and reliable. Cement-bonded wood wool board was made in Austria from about 1908, under names such as Heraklith.

Source: content/entries/knowledge/wood-pulp-and-paperboard.md