◆ Rebuild

Part 3 · Metals

Antimony and Bismuth

Two brittle, low-melting metals that are almost useless alone and indispensable in alloys. Antimony hardens lead and tin into type metal, bearing metal, pewter and battery plates; bismuth makes alloys that melt in boiling water. This chapter covers finding their ores, sweating stibnite out of its rock, reducing it with iron, and handling both safely.

Difficulty
●●●●●
Time
An afternoon to test an ore; a day to liquate a batch; half a day per crucible reduction
Steps from zero
3 prerequisites →

You need first

Finding and Identifying OresCharcoal

This unlocks

—

Objects made here

liquation pottype metal
The full path from nothing — 3 steps before this one
  1. Fire
  2. Finding and Identifying Ores
  3. Charcoal
  4. Antimony and Bismuth

Do them roughly in this order. See it on the tech tree →

Why it matters

Neither metal makes a tool. Antimony is as brittle as glass — you can crush a lump in a mortar — and bismuth is not much better. But a little of either changes other metals completely:

  • Type metal. Lead with about 15% antimony and some tin is hard, casts sharp letters, and swells slightly as it sets, filling every corner of the mould. Without it, cast type for Printing is soft and blurred.
  • Bearing metal. Tin or lead holding hard crystals of antimony and copper is babbitt, the lining of every good shaft bearing in an engine or mill (Bearings and Lubrication).
  • Pewter and Britannia metal. 6–8% antimony makes tin stiff enough to spin into thin cups and plates, with no lead at all (Tin and Pewter).
  • Hard lead. A few percent antimony stiffens lead sheet and pipe, and the grids of the The Rechargeable Battery.
  • Solders. Tin with 5% antimony is a strong lead-free solder for water pipes; tin with 58% bismuth melts at only 138 °C (Soldering and Brazing).
  • Fusible alloys. Bismuth, lead and tin together melt below the boiling point of water. That gives safety plugs for boilers and canners, a filling for bending thin tubes without kinking them, and a way to cast fine detail.

Both are small trades. A whole printing shop needs only a few kilograms of antimony; a community might need a few kilograms of bismuth in a generation. But when you need them, nothing else does the job.

How it works

Antimony and bismuth sit between metals and non-metals. They conduct electricity poorly, they are brittle, and — unusually — both expand when they freeze, as water does. That is why they make alloys that fill moulds sharply.

Antimony Bismuth
Colour Bright silver-white with a bluish tinge Silver-white with a pinkish tinge; tarnishes in rainbow colours
Melts at 631 °C (dull red) 271 °C (below red heat — melts in a candle flame)
Density (water = 1) 6.7 9.8 (nearly as heavy as lead)
Main ore Stibnite (antimony sulfide) Native bismuth (the metal itself); bismuthinite (sulfide)
Poisonous? Yes, rather like arsenic, less severe Only mildly; the least poisonous heavy metal

Getting antimony out of stibnite uses three facts:

  1. Stibnite melts at about 550 °C, long before the quartz and rock it sits in. Heated gently in a pot with holes in the bottom, it sweats out and drips away from its rock. This is liquation. The product, purified stibnite, was sold for centuries as "crude antimony".
  2. Iron grabs sulfur more strongly than antimony does. Melt stibnite with iron scrap and the iron takes the sulfur, becoming a dark, light iron sulfide (matte), while heavy metallic antimony sinks to the bottom: stibnite + iron → antimony + iron sulfide. This is iron precipitation, the oldest and simplest route.
  3. Antimony fumes easily in air. Roasted or overheated with air, stibnite turns to a white smoke of antimony oxide, which is both poisonous and lost metal. So every step is done with little air and no more heat than needed.

Bismuth is easier. It is often found as native metal in its ore, and it melts at only 271 °C, so it simply runs out of crushed ore warmed on a fire.

Wind at your backfumes blow away from you Clay lidsealed round with wet clay Ring of fireround the upper pot only;dull red, 550–650 °C Stibnite orewalnut-sized lumps Floor with holes6–10 holes, 1 cm across Clay sealkeeps air out Lower potburied to the rim, stays cool Crude antimonygrey cake of pure stibnite Molten stibnite drips through the holes; quartz and rock stay behind in the upper pot.
Fig. 1 Liquation of stibnite. Ore sits in an upper pot with holes in its floor; a fire round the upper pot only melts the stibnite, which drips into a lower pot kept cool in the ground.

What you need

Item Amount Notes
Stibnite ore 10–50 kg for a batch Rich lumps, hand-picked; see below
Clay pots Pairs: an upper pot of 5–10 litres with 6–10 holes of 1 cm in the floor, and a lower pot of 2–4 litres Ordinary fired Pottery, with sand or grog in the clay (Firebrick and Refractories)
Crucible with lid Holds 2–5 kg Fireclay and grog (Firebrick and Refractories); for the reduction
Iron scrap 40–45 parts per 100 parts of liquated stibnite Nails, filings, cut-up wire, bloomery scraps — small and clean (Iron (the Bloomery))
Flux About 10 parts per 100 of stibnite Common Salt, or Soda Ash and Baking Soda, or potash from Lye and Potash-making
Charcoal 10–20 kg per batch Charcoal
Forge or wind furnace Reaching bright red, about 1,000 °C Bellows, The Kiln
Cone mould Iron or stone, a cone 8–12 cm deep, point down Smeared with clay wash or chalk so the metal releases
Hammer, tongs, iron rod Blacksmithing

Where to find it

Stibnite forms in quartz veins and around old hot springs, often in the same districts as gold, mercury (cinnabar) and arsenic minerals (realgar and orpiment). Big deposits are known in southern China (Hunan), Bolivia, Turkey, the Balkans, Algeria and Japan, and small veins in many old mountain belts. Look for:

  • Long, lead-grey, very shiny crystals like needles or flat sword blades, often in radiating sprays or tangled masses, with fine lines running along their length.
  • Soft — a knife cuts it easily and it leaves a dark grey mark on paper.
  • Light for a metallic mineral — noticeably lighter in the hand than galena, which it resembles. Galena breaks into little cubes; stibnite into long splinters.
  • Yellow and white crusts (antimony ochres) where it weathers at the surface, often on rusty quartz.
  • The candle test. Hold a thin splinter in a candle flame with tweezers or a split stick. Stibnite melts and beads up, giving off white fumes (hold it at arm's length outdoors and do not breathe them). Galena does not melt in a candle. Bismuthinite may also melt, so tell it apart by weight (below).

Bismuth is rarer. It turns up in veins with tin, tungsten, silver, cobalt and nickel ores — classic districts are the Ore Mountains of Saxony and Bohemia, Cornwall, Bolivia, Peru and Australia — and is often a by-product of mining those metals.

  • Native bismuth: silver-white metal with a pinkish cast, very heavy, brittle, breaking along shiny flat faces; old surfaces tarnish to iridescent pink, blue and gold. A chip melts at once in a candle flame to a bright bead.
  • Bismuthinite: looks like stibnite (grey needles) but is much heavier in the hand (density about 6.8 against stibnite's 4.6). Do not rely on the candle test to tell them apart.
  • Bismuth ochre: soft yellow or greenish-yellow earthy crusts on bismuth-bearing veins.

Warning Many antimony and bismuth ores carry arsenic minerals, and cobalt-bismuth ores nearly always do. Strike a sample with a steel hammer and sniff from a distance: a smell of garlic means arsenic. Read Arsenic before you heat any of it.

Method 1: Liquating stibnite

Do this outdoors, on open ground well away from homes, wells and gardens, with the wind at your back.

  1. Sort the ore. Break it with a hammer to lumps the size of a walnut (2–4 cm). Pick out lumps that are mostly grey stibnite; throw back pieces that are mostly white quartz or rust. Liquation is worth doing only on rich ore — roughly a third or more stibnite by weight. Leaner ore must be crushed, washed like gold or tin ore (Finding and Identifying Ores) and smelted in the crucible directly.
  2. Set the lower pots in a row of holes in the ground so that their rims are level with the surface. Packing earth round them keeps them cool, so the stibnite freezes as it arrives and does not boil away.
  3. Set an upper pot on each, mouth to mouth, with its perforated floor resting on the lower pot's rim. Seal the joint with a ring of wet clay so air cannot get in.
  4. Fill the upper pots with the sorted lumps and put on a clay lid, luted (sealed) round with clay.
  5. Build a ring of fire round the upper pots only — wood or charcoal — and keep it burning for 1½–3 hours. The pots should reach a dull red, just visible in shade (about 550–650 °C). No brighter: too hot and the stibnite fumes, and the clay may crack.
  6. Let it all cool for several hours. Lift off the upper pots: the spent rock in them is mostly quartz, and can be thrown away or crushed and washed for the last scraps. In each lower pot is a cake of shiny grey crude antimony — purified stibnite — with long bladed crystals on its broken face.

Expect 30–60% of the stibnite to come out on a first try; better ore and patient, even heating give more.

Method 2: Reducing with iron

This turns stibnite into metal. One crucible charge gives about 1–3 kg of antimony.

1. Melt 2. Pour into a cone 3. Refine and "star" Slagglassy Matteiron sulfide Antimonyregulus Lidded crucible, bright red, about 1,000 °C, 30–60 minutes. Charge by weight: 100 stibnite, 40–45 iron scrap, 10 salt or soda. Iron scrap at the bottom, the rest on top. Heaviest settles lowest. Break it out when cold; keep the bright button at the tip. Remelt the matte with fresh stibnite to recover more. Remelt with 1/10 stibnite and 1/10 soda; cool without moving. Fern-like leaves on the top face mean pure antimony. A smooth, dull face means iron or sulfur remains.
Fig. 2 Reducing stibnite with iron. The charge melts in a lidded crucible; poured into a cone mould, the heavy antimony sinks to the tip under a layer of iron sulfide matte and slag. Remelted under a flux and cooled slowly, pure antimony shows a fern-like "star" on its top face.
  1. Weigh the charge, by weight: 100 parts crude antimony (crushed to pea size), 40–45 parts small iron scrap, about 10 parts salt or soda ash. For example, 3 kg stibnite, 1.3 kg iron, 300 g salt. The flux makes a runny slag that helps the drops of metal fall through.
  2. Heat the crucible empty to red, in a forge or wind furnace. Add the iron first, then the stibnite and flux on top, and put the lid on.
  3. Bring it to a bright red, about 1,000 °C, and hold it there for 30–60 minutes, until a dry iron rod pushed in meets no lumps and comes out coated with thin liquid. Small blue-white flames and a little white smoke at the lid are normal; thick white smoke means too much air or too much heat — close the furnace down a little.
  4. Warm the cone mould till it is too hot to touch, so no moisture remains, and set it on dry sand.
  5. Pour the whole melt into the cone in one smooth movement. Let it cool for an hour.
  6. Knock it out and break it with a hammer. At the tip is a heavy, bright, silvery regulus (button) of antimony with a coarse crystalline fracture. Above it lies a dark bronze-coloured, lighter iron sulfide matte, and on top a glassy slag. Separate the regulus. Save the matte: crushed and remelted with a little fresh stibnite, it gives up more antimony.

From 100 kg of pure stibnite you can hope for about 55–65 kg of antimony (it contains 72%).

Refining and "starring"

The first regulus holds a few percent of iron and sulfur, which make it dull and spoil alloys.

  1. Remelt the regulus with about one-tenth of its weight of fresh crude antimony and one-tenth of soda ash or potash, at a steady red, for 20–30 minutes. The added stibnite takes up the leftover iron.
  2. Pour into a warm mould and let it cool without moving it at all, under its skin of slag.
  3. Look at the top face. Pure antimony freezes with a beautiful pattern of fern-like leaves or stars on its surface — the old "star antimony". If the face is smooth and dull, repeat the remelt.

Method 3: Bismuth

  1. Native bismuth ore: crush to hazelnut size and spread it on an iron pan or a sloping trough of fired clay, over a gentle charcoal fire, under a lid or a layer of charcoal dust. At about 300 °C — not yet glowing, but hot enough to char a stick laid on it — the bismuth melts and runs out of the rock to the low end. Historically the Saxon miners did this in sloping iron tubes over a fire, letting bismuth trickle out of the bottom into an iron dish.
  2. Bismuthinite (sulfide) is reduced with iron exactly as stibnite is, using 100 parts ore to about 25–30 parts iron.
  3. Bismuth ochre (oxide) is reduced in a crucible with one-fifth of its weight of powdered charcoal and a little soda, at a dull-to-bright red. Bismuth sinks; pour it off into a mould.
  4. Clean it by remelting under charcoal dust and skimming. Pure bismuth that is melted, allowed to grow a crust, and then has the liquid poured out from under the crust leaves hollow, stepped crystals inside — the famous "staircase" crystals.

Using them: alloys

Always melt the highest-melting metal first, then add the others; stir with a dry green stick and skim. Add antimony broken small and wrapped in tin foil, and push it under the surface with the stick, so it dissolves instead of floating and fuming.

Alloy Parts by weight Melts at Use
Type metal Lead 70–80, antimony 15–20, tin 5–10 240–260 °C Cast type (Printing)
Tin babbitt Tin 89, antimony 7–8, copper 3–4 about 240–360 °C Engine bearings (Bearings and Lubrication)
Lead babbitt Lead 80, antimony 15, tin 5 about 240–270 °C Slow shafts (Bearings and Lubrication)
Britannia metal Tin 92, antimony 6, copper 2 about 250–300 °C Spun cups, plates, teapots (Tin and Pewter)
Hard lead Lead 94–97, antimony 3–6 about 300 °C Battery grids, stiff sheet
Antimony solder Tin 95, antimony 5 232–240 °C Lead-free water-pipe joints
Tin–bismuth solder Bismuth 58, tin 42 138 °C Low-heat solder; joints near heat-sensitive parts
Rose's metal Bismuth 50, lead 25, tin 25 about 95–98 °C Fusible plugs; tube bending; fine castings

Bending a thin tube with a fusible alloy. Plug one end of a copper or brass tube with clay, fill it with melted Rose's metal, let it set, bend the tube round a former — the filling stops it kinking — then drop it in boiling water. The alloy melts and pours out to be used again. Do this only for tools and instruments, never for food or water fittings: it contains lead.

Tip To check the composition of an alloy without instruments, cast a small bar of a known good mix and keep it. Compare a fresh casting by its fracture, its hardness under a file, and the sharpness of its cast corners.

How to tell it worked

  • Antimony is bright, bluish-white and very brittle: a light hammer blow shatters it into shiny crystalline flakes. A file skates on it. Heated on charcoal in a blowpipe flame it melts and gives off white fumes (test only a crumb, outdoors).
  • Star pattern on a slowly cooled top face means good purity.
  • Bismuth is pinkish-white, very heavy for its size, and melts on a hot iron at a heat that only scorches paper.
  • The alloy test. A good type metal casting has sharp corners and a fine grey fracture; a good babbitt scratches but does not crumble; Rose's metal melts in a pot of boiling water.

Note Troubleshooting. Thick white smoke during liquation → fire too hot, or air getting into the pots. Damp the fire down and seal the joints better. Nothing ran out of the upper pot → not hot enough, or the ore was too lean. Hold a dull red longer; crush and wash lean ore. No regulus at the cone tip, only matte → too little iron, or too cool to separate. Add 10% more iron and heat longer and brighter. Regulus is dull and rough, no star → still iron or sulfur in it. Remelt with fresh stibnite and soda. Antimony floats on the alloy melt and burns → push it under, wrapped in tin foil, and cover the pot with charcoal. The bismuth smells of garlic when heated → it carries arsenic. Stop, and see Arsenic.

Dangers

Danger Antimony fumes and dust are poisonous, and stibnite ores often bring arsenic with them. The white smoke from roasting, liquating or overheating antimony irritates the lungs, eyes and skin, and repeated exposure damages the heart, lungs and stomach. Work outdoors, upwind, away from water and food stores; keep children and pregnant women away. Never deliberately roast stibnite in open air to make the oxide — it gives off the most fume of all.

Danger Stibine gas. Antimony or antimonial lead in contact with acid that is giving off hydrogen — for example a lead-acid battery being charged hard, or scrap being dissolved in acid — can release stibine, a deadly gas. Charge batteries in a well-aired place, and never treat antimony alloys with acid indoors.

  • Molten metal and water. As with all casting: dry pots, dry moulds, dry tools (Metal Casting).
  • Never use antimony for food or drink vessels. In the 1600s and 1700s people kept "antimony cups": wine left standing in one dissolved enough antimony to make the drinker vomit, and the dose was easily fatal. Britannia metal is safe only because the antimony is locked in a tin alloy and is a small part of it.
  • Bismuth is far less poisonous than lead or antimony, but its fumes still should not be breathed, and fusible alloys contain lead: wash your hands.

What this unlocks

Type metal for Printing. Babbitt for Bearings and Lubrication in mills, the The Steam Engine and Machine Tools. Lead-free pewter for tableware (Tin and Pewter). Stiff grids for the The Rechargeable Battery. Fusible safety plugs for the boilers of Canning and Bottling and steam plant. Antimony sulfide also goes into the heads of some Matches, and lead antimonate makes a warm yellow pigment (Pigments, Paints and Varnish). Much later, both metals are ingredients of Semiconductors and the Transistor.

How it was first done

Powdered stibnite was ground into kohl, the black eye paint of ancient Egypt and the Near East, for thousands of years; some ancient "kohl" turns out on analysis to be galena instead. A few objects of metallic antimony survive from early Mesopotamia, but the metal stayed a curiosity. The Italian metalworker Vannoccio Biringuccio described liquating and reducing antimony in his Pirotechnia (1540), and in the 1600s alchemical books such as the Triumphal Chariot of Antimony made it famous — and dangerous, as a fashionable medicine. Type founders in Europe were using lead-tin-antimony alloys from the early centuries of printing; antimony was found in some of the earliest surviving European type.

Bismuth was mined in the Ore Mountains of Saxony by the 1400s and is described by Georgius Agricola in 1546, but for a long time it was confused with lead and tin. The French chemist Claude Geoffroy showed in 1753 that it was a metal in its own right. Fusible alloys of bismuth, lead and tin were studied by Isaac Newton and others around 1700, and Valentin Rose's version gave its name to Rose's metal.