◆ Rebuild

Part 2 · Earth and Fire

Synthetic Gems

Sprinkle pure alumina powder through an oxygen–hydrogen flame and it melts, drop by drop, onto a growing crystal of ruby or sapphire — the Verneuil process. It turns a few kilograms of alum into the jewel bearings of watches, meters and compasses, scratch-proof windows and top-grade abrasive. In outline, how quartz crystals are grown from hot alkaline water under great pressure when natural rock crystal runs out.

Difficulty
●●●●●
Time
Weeks to purify alum and build the burner; 4–8 hours per boule; months to learn to make clear, unbroken boules and turn them into jewels
Steps from zero
24 prerequisites →

You need first

Gem Cutting and LapidaryHydrogen, Oxygen and Gases

This unlocks

—
The full path from nothing — 24 steps before this one
  1. Stone Tools
  2. Fire
  3. Cordage and Rope
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Abrasives and Grinding Stones
  9. Charcoal
  10. Pottery
  11. The Kiln
  12. Hides and Leather
  13. Gem Cutting and Lapidary
  14. Salt
  15. Lime
  16. Fermentation
  17. Lye and Potash
  18. Glass
  19. Bellows
  20. Copper Smelting
  21. Laboratory Glassware
  22. The Battery
  23. Electrolysis
  24. Hydrogen, Oxygen and Gases
  25. Synthetic Gems

Do them roughly in this order. See it on the tech tree →

Why it matters

Ruby and sapphire are both corundum — crystalline aluminium oxide — the hardest common substance after diamond. A steel pivot turning in a corundum bearing runs for decades without wear (Watches and Small Clocks, Measuring Electricity, The Compass). Natural corundum is rare, small and full of cracks. Flame fusion makes it by the kilogram, clear and flawless, from clay and acid.

What synthetic corundum gives you:

  • Jewel bearings — the hole jewels and cup jewels of watches, clocks, electric meters, compasses and every fine instrument (Scientific Instrument Making).
  • Wear parts — thread guides that cotton and silk cannot cut (Textile Machinery), knife-edges for balances, gauge tips, nozzles.
  • Windows that sand and grit cannot scratch, and that stand red heat.
  • Abrasive — crushed scrap boules are grit as hard as the best emery (Abrasives and Grinding Stones).
  • Gems — rubies and sapphires chemically identical to natural ones (Jewellery, Beads and Medals).

Cultured quartz matters for a different reason: every radio transmitter and quartz clock needs perfect, untwinned rock crystal (Quartz Crystals and Frequency Control), and natural crystal of that quality runs out quickly.

How it works

Flame fusion

Alumina melts at about 2,050 °C — far beyond any fuel furnace. A jet of hydrogen burning in oxygen reaches about 2,800 °C (Hydrogen, Oxygen and Gases).

The trick, found by Auguste Verneuil, is to melt the powder a little at a time, on top of the crystal itself:

  1. Very fine alumina powder is shaken, a pinch at a time, into the oxygen stream of a burner pointing straight down.
  2. The grains melt as they fall through the flame.
  3. They land on the top of a pedestal, where a thin cap of melt sits on a solid crystal.
  4. The pedestal is lowered slowly, as fast as the crystal grows, so the cap stays at the same hot spot. Below the cap, the melt freezes onto the crystal underneath, copying its order atom for atom.

The result is a single crystal shaped like a carrot or a pear: a boule (French for "ball").

hopper of powder pure alumina + chromium oxide fine sieve hydrogen in outer tube; meets oxygen only at the nozzle water-cooled nozzle fireclay muffle 8–10 cm inside pedestal fireclay or alumina rod cam-driven tapper 20–80 taps a minute oxygen in carries the powder down the central tube oxyhydrogen flame sight hole molten cap kept at one height ruby boule single crystal, 15–25 mm wide lowering screw 5–10 mm an hour
Fig. 1 The Verneuil furnace. A tapper shakes alumina powder through a sieve into the oxygen stream; hydrogen joins it at the nozzle; the flame burns downward into a fireclay muffle, where a ruby boule grows on a pedestal that is screwed slowly down.

Colour

Pure corundum is colourless ("white sapphire"). Traces of other oxides colour it:

Add to the alumina Colour
Chromium oxide, about 0.1–0.5% Pink
Chromium oxide, about 1–3% Ruby red
Iron oxide and titanium oxide, a few tenths of a per cent each Blue sapphire
Nothing Colourless

Watch jewels are usually ruby: the red makes tiny pieces easy to see and handle, and chromium does no harm to hardness.

What you need

Item Amount / size From
Ammonium alum, recrystallised 3–4 times About 10 kg per kg of alumina Clay or alum shale and Sulfuric Acid; ammonia (Ammonia)
Chromium oxide or chrome alum (for ruby) A few grams per 100 g alumina Chromite ore (Chromium and Its Compounds)
Hydrogen and oxygen Several cubic metres per boule Electrolysis of water (Hydrogen, Oxygen and Gases) or liquid air (Liquid Air, Nitrogen and the Noble Gases); gas holders
Burner Brass and copper tubes, water-cooled tip Metal Pipes and Tubes, Soldering and Brazing
Muffle Fireclay tube 8–10 cm inside, 25–30 cm tall Firebrick and Refractories
Lowering screw A fine screw turned by clockwork or a slow motor Screws, Nuts and Bolts, The Mechanical Clock
Dark glass To watch the flame Smoked or cobalt-blue glass (Glass)
Cutting Diamond powder if you have any; otherwise carborundum The Electric Arc Furnace, Abrasives and Grinding Stones

Where to find it

  • Alumina comes from any clean white clay (kaolin) or alum shale — dark, papery shale that grows white, sour-tasting crusts as it weathers (Aluminium, Finding and Preparing Clay).
  • Chromite is black, heavy, weakly magnetic, with a dark brown streak, found in dark green serpentine country (Chromium and Its Compounds).
  • Ilmenite for blue sapphire comes from black beach sand (Titanium).
  • Natural corundum pebbles from gem gravels are useful as seed crystals, though any boule fragment works (Gem Cutting and Lapidary).

Step 1: Make the powder

The powder must be pure, dry, very fine and light, so it trickles evenly and melts instantly. Ordinary alumina from bauxite (Aluminium, Alum and Alumina) is too coarse and gritty. Verneuil's answer was ammonium alum, because when roasted it leaves nothing but alumina.

  1. Aluminium sulfate. Dissolve the alumina out of calcined white clay with hot dilute sulfuric acid, as in Alum and Alumina. Filter.
  2. Ammonium alum. Stir in ammonium sulfate (ammonia neutralised with sulfuric acid — Chemical Fertilisers), about 1 part to 4 parts of aluminium sulfate by weight. Cool: clear, eight-sided alum crystals grow. Use ammonium alum, not potash alum — potassium stays behind in the powder and spoils the crystal.
  3. Purify. Dissolve the crystals in the least hot clean water, and cool them again. Repeat three or four times, using rain or distilled water (Distillation). Any iron left will tint the boule brown.
  4. Chromium (for ruby). Only a few grams are needed. Green chromium oxide and violet chrome alum are made from chromite ore by a route that passes through yellow chromate, a cancer-causing form of chromium; that route and its precautions are in Chromium and Its Compounds. The best way to spread the chromium evenly is to crystallise a little chrome alum together with the ammonium alum in the last recrystallisation; otherwise grind the oxide very fine and mix it in thoroughly.
  5. Calcine. Put the purified alum (with its chromium, mixed well) in a clean clay dish and heat it slowly: it melts in its own water, swells into a huge white sponge, then gives off ammonia and choking white sulfur trioxide fumes. Finish at 1,000–1,100 °C (yellow heat) for 2–3 hours.
  6. Grind gently and sieve through the finest cloth. Good powder is white (pale pink for ruby), light as flour, and flows like dry talc.

Step 2: Build the furnace

  1. The hopper. A brass cylinder 5–8 cm across with a fine metal-gauze sieve for a bottom (about 40 wires per centimetre), holding 100–200 g of powder. A small hammer, lifted by a cam and dropped, taps the top of the hopper 20–80 times a minute. More taps, more powder. Drive it by clockwork or a small motor.
  2. The burner. Below the hopper, the oxygen enters and carries the falling powder down a central tube 5–8 mm across. Round it, an outer tube carries hydrogen. The two gases meet only at the nozzle. Wrap the nozzle in a coil of copper tube with cooling water running through it, or it will melt.
  3. The muffle. The flame burns downward into a fireclay tube 8–10 cm across, with a small sight hole (covered with mica or glass) at the level of the crystal top.
  4. The pedestal. A fireclay or alumina rod about 1 cm thick stands up inside the muffle, on a carriage moved by a fine vertical screw. Turned by clockwork, it lowers the pedestal steadily, about 5–10 mm an hour, with a hand wheel to adjust.
  5. Gas supply. Hydrogen and oxygen from separate gas holders at steady low pressure, each through a water-bottle flashback trap and a needle valve (Hydrogen, Oxygen and Gases). Use more hydrogen than oxygen — about 2½ to 3 volumes of hydrogen to 1 of oxygen — so the flame is not oxidising. Very roughly, a small burner uses half a cubic metre or more of hydrogen an hour.
1. Boule 2. Split 3. Slice wafers 4. Round discs 20 mm × 50 mm,about 300 carats splits along its lengthfrom cooling strain 0.5–1 mm thick, cut withdiamond or carborundum faces lapped flat;hole drilled from both sides Hole jewel (cut through) Cup jewel (cut through) hole rounded ("olived"), touches pivot in the middle steel pivot 0.1–0.5 mm brass seat compass needle conical pit 60–90°, blunter than the point disc 2–4 mm across
Fig. 2 From boule to jewel. The cooled boule is split along its length, sawn into thin wafers, cut into small squares, ground round, drilled, opened and polished into hole jewels, or ground with a conical pit for a cup jewel.

Step 3: Grow a boule

  1. Light the hydrogen first, then turn on the oxygen slowly until the flame is a short, quiet, pale blue jet. Let the muffle heat for 20–30 minutes.
  2. Start the powder. Tap slowly. A cone of white sintered powder builds on the pedestal.
  3. Melt the tip. Raise the oxygen a little and lift the pedestal until the tip of the cone melts into a small, glowing, round drop. Look through dark glass: the melt shines blinding white-yellow.
  4. Make a neck. Lower the pedestal a little and keep the feed slow, so that the crystal grows thin — a stalk 2–3 mm across for the first centimetre. Many tiny crystals start at the tip; in a thin neck, one usually crowds out the rest. (Better: start on a small seed — a sliver of a previous boule set in the pedestal.)
  5. Widen. Slowly increase the tapping and the gases so the top spreads out to the full width you want, 15–25 mm. Then hold everything steady.
  6. Grow. Keep the molten cap at exactly the same height, just under the bright inner cone of the flame, by turning the lowering screw. The cap must stay a thin, round, shining dome. Grow for 4–8 hours: a boule 50–60 mm long.
  7. Finish. Stop the powder, then reduce the oxygen and hydrogen gradually over 10–15 minutes so the boule cools slowly in the muffle.

A boule of 20 mm by 50 mm weighs about 60 g — 300 carats. It is full of strain and often splits lengthwise into two halves as it cools, or when tapped gently with pliers at its base. This is normal and does not spoil it.

Step 4: From boule to jewel

Corundum is cut only by something harder. Diamond powder (from crushed industrial diamond) in oil is best. Without it, use carborundum (silicon carbide from the The Electric Arc Furnace) or boron carbide: slower, but it works. The methods are those of Gem Cutting and Lapidary at smaller scale.

  1. Slice the half-boule into wafers 0.5–1 mm thick with a thin soft-iron or copper disc charged with the grit, running in oil.
  2. Cut squares a little bigger than the finished jewel. Cement them in rows with shellac onto a flat plate and grind both faces flat and to thickness on a cast-iron lap, as for crystal plates (Quartz Crystals and Frequency Control).
  3. Round them: thread many squares on a wire through a rough hole, or cement them in a stack, and grind the stack round on the lathe.
  4. Drill the hole jewels with a fine steel needle charged with diamond powder, worked from both sides. Watch jewels have holes of only 0.1–0.2 mm; instrument jewels 0.2–0.5 mm. Then open the hole with a fine wire coated in grit, drawn back and forth, and round ("olive") its walls so the pivot touches only in the middle.
  5. Cup jewels for compass needles and meter pointers are discs 2–4 mm across with a conical pit a little blunter than the pivot point (about 60–90°), ground with a pointed steel tool and grit, then polished (Gem Cutting and Lapidary).
  6. Polish every working face with the finest diamond or tin-oxide on a hard wooden lap until it shows no scratch under a strong lens.
  7. Set them by pressing into a reamed brass seat or burnishing a brass rim over them (Watches and Small Clocks).

Other flame-fusion crystals

The same furnace grows spinel (alumina with magnesia — Magnesium), and rutile from pure titanium dioxide (Titanium), a gem with more fire than diamond but much softer. Crushed boule scrap is excellent abrasive. For grit by the tonne, bauxite melted in the arc furnace gives fused alumina directly (The Electric Arc Furnace, Abrasives and Grinding Stones).

Growing quartz (in outline)

Quartz cannot be grown from its melt: molten silica cools to glass, not crystal (Pure Silicon). Instead it is dissolved in hot water under great pressure and laid down again on seed plates — the way quartz veins form deep in the earth.

sealed plug with bursting disc thick forged steel wall ≥ inside radius seed plates thin slices of perfect quartz; new quartz grows on them baffle perforated plate nutrient crushed clear quartz, dissolves in the hot zone caustic soda solution fills about 80% of the space; 700–1,500 atmospheres when hot cooler heater 20–40 °C below the bottom hotter heater 350–400 °C Run 1–2 months, in a pit or behind an earth wall.
Fig. 3 The hydrothermal autoclave in outline. A thick steel vessel holds alkaline water. Crushed quartz in the hotter bottom dissolves; the solution rises through a baffle to the cooler top, where quartz grows on thin seed plates.
  • The vessel is a thick-walled forged alloy-steel cylinder (Alloy and Stainless Steels) — for a small one, perhaps 5–10 cm inside and 50–100 cm long, with walls at least as thick as the inside radius and a screwed or sealed plug.
  • The bottom holds crushed clear quartz, the nutrient. A perforated steel baffle across the middle steadies the flow.
  • The top holds seed plates — thin slices of perfect quartz cut in a chosen direction (Quartz Crystals and Frequency Control) — hung on silver or steel wire frames.
  • The solution is weak caustic soda or sodium carbonate (about 1 mole per litre — Lye and Potash, Soda Ash and Baking Soda), filling about 80% of the free space. The filling decides the pressure.
  • Heat the bottom to about 350–400 °C and keep the top about 20–40 °C cooler. The pressure rises to roughly 700–1,500 times atmospheric. Quartz dissolves in the hot zone, the solution rises, and in the cooler zone it is over-full and quartz grows on the seeds, perhaps 0.5–1 mm a day on the fastest face.
  • A run lasts one to two months. The crystals come out as clear, bar-shaped blocks, ready to saw into oscillator plates.

This needs forged alloy steel, high-pressure seals, steady furnaces controlled to a few degrees and a pressure gauge for a thousand atmospheres. It is a project for a settlement that already builds high-pressure boilers (Boilers and Pressure Vessels) and synthetic ammonia plants (Ammonia).

How to tell it worked

  • Corundum scratches quartz, topaz and hardened steel easily, and is scratched only by diamond and carborundum. It weighs about 4 times its volume of water. A good boule is clear and evenly coloured all through.
  • Synthetic, not natural. Under a strong lens, flame-fusion corundum shows curved growth lines, like the grooves of a record, and sometimes tiny round gas bubbles. Natural stones show straight growth bands and angular crystal inclusions. Always sell synthetic stones as synthetic.
  • Ruby glows red under ultraviolet light, such as the light of a carbon arc seen through dark violet glass, and in strong blue light.
  • Jewels: a pivot turns in a jewel with no grating; under a lens the hole is round, smooth and centred.

Note When it goes wrong. Boule cloudy or white → powder too coarse, feed too fast, or the cap is too cool. Tap less, raise the oxygen slightly. Many crystals instead of one (a crusty, grainy boule) → neck too thick or no seed. Make a thinner neck or use a seed. Boule brown or yellow → iron in the alum. Recrystallise more times. Melt drips off the side → cap too hot or too wide; reduce oxygen or lower the pedestal. Boule shatters into pieces → cooled too fast; reduce the gases more slowly, and keep the muffle closed. Burner tip melts → cooling water failed. Always check the water flows before lighting.

Dangers

Danger Hydrogen explodes. A hydrogen–oxygen mixture in a pipe, a gas holder or the muffle can blow up with the force of a bomb. Never mix the gases before the nozzle. Fit a water-bottle flashback trap on each line. Always light the hydrogen first and turn off the oxygen first. Purge the muffle with hydrogen before lighting. See Hydrogen, Oxygen and Gases.

Danger Pressure vessels kill. A quartz autoclave holds the energy of a large explosive charge. Test every vessel full of cold water to one and a half times its working pressure first. Run it in a pit or behind a thick earth wall, fit a bursting disc, and never stand near it or try to open it while it is hot or under pressure.

  • Eyes. The melt is as bright as an arc. Look only through dark glass, and never into the flame without it.
  • Calcining alum gives off ammonia and sulfur trioxide fumes that burn the lungs: outdoors, upwind.
  • Chromates cause skin ulcers and cancer (Chromium and Its Compounds). Use only the green or violet forms at the furnace; never pour chromate on the ground or into water.
  • Hot caustic in an autoclave blinds instantly (Lye and Potash).

What this unlocks

Jewelled bearings make watches and portable timekeepers last (Watches and Small Clocks), and give the low-friction pivots of sensitive meters (Measuring Electricity), compasses (The Compass) and balances. Corundum thread guides and wear parts serve Textile Machinery and the The Sewing Machine. Cultured quartz supplies every quartz oscillator for Radio, clocks and The Computer timing. A rod of synthetic ruby, mirrored at both ends and lit by a bright flash, was the first laser (1960).

How it was first done

In 1877 the French chemists Edmond Frémy and Charles Feil grew tiny ruby crystals by dissolving alumina in molten salts. Around 1885 crude flame-melted "Geneva rubies" appeared on the market, full of bubbles and strain. Frémy's assistant Auguste Verneuil solved the problem with the downward oxyhydrogen burner and slow lowering of the boule; he announced it in 1902 and published the full method in 1904. Within a few years factories in France, Switzerland and Germany were making millions of carats a year, and Swiss watches became fully jewelled. When the Second World War cut the United States off from European jewels, the Linde company began making Verneuil sapphire there.

Quartz was first grown on seed crystals in hot water under pressure by Giorgio Spezia in Turin in the early 1900s. During the Second World War Richard Nacken in Germany and, after it, Bell Telephone Laboratories and the Brush Development Company in the United States developed the process for oscillator crystals. By the late 1950s cultured quartz was replacing natural Brazilian crystal in radio and telephone equipment, and today almost all oscillator quartz is grown.

Source: content/entries/earth/synthetic-gems.md