A membrane is a sieve so fine that it can stop germs, then viruses and proteins, and finally the salt dissolved in sea water. This chapter climbs that ladder from folded cloth and fired clay filters to cellophane and cellulose acetate films, explains osmosis and how pumping against it gives fresh water from brackish wells and the sea, and shows the other road to fresh water, boiling sea water in solar stills and multistage flash plants. It ends with dialysis membranes, which clean blood, in outline.

Difficulty
●●●●●
Time
A week to make and fire ceramic filters; months of trials to cast working salt-rejecting membranes; years and a chemical industry for a seawater plant
Steps from zero
41 prerequisites →

You need first

Water Softening and Ion ExchangePetrochemicals and Modern Plastics

This unlocks

Kidney Dialysis
The full path from nothing — 41 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Measurement from Scratch
  8. Writing and Numbers
  9. Hunting and Trapping
  10. Basic Woodworking
  11. Pottery
  12. The Kiln
  13. Charcoal
  14. Arithmetic and Fractions
  15. Hides and Leather
  16. Tiles and Clay Pipes
  17. Salt
  18. Lime
  19. Surveying and Levelling
  20. Fermentation
  21. Lye and Potash
  22. Glass
  23. Bellows
  24. Saltpeter
  25. Distillation
  26. Lead
  27. Copper Smelting
  28. Iron (the Bloomery)
  29. Sulfuric Acid
  30. Blacksmithing
  31. Pipes, Plumbing and Aqueducts
  32. Nitric Acid
  33. The Battery
  34. Steel
  35. Early Plastics
  36. Electrolysis
  37. Chlorine and Bleach
  38. Petroleum and Refining
  39. Water Treatment for a Town
  40. Petrochemicals and Modern Plastics
  41. Water Softening and Ion Exchange
  42. Membranes, Reverse Osmosis and Desalination

Do them roughly in this order. See it on the tech tree →

Why it matters

Most water problems are problems of separation: the water carries mud, germs, viruses or salt. Earlier chapters deal with them by settling, sand and chlorine (Water Treatment for a Town), ion exchange (Water Softening and Ion Exchange) and boiling (Distillation). A membrane separates by size alone, with no chemicals and no fire. A wall of fired clay stops bacteria. A film of cellulose stops viruses and proteins. A film of cellulose acetate or polyamide, pressed hard enough, lets water through and holds back the salt of the sea. That gives germ-free water from a clay pot in every house; fresh water from the brackish wells under much of the world's dry land, with a pump a person can pedal; fresh water from the sea for islands and deserts; sterile liquids that cannot be boiled (Making Medicines, Culturing Microbes); very pure water for boilers and chips (Making Microchips); and clean blood for people whose kidneys have failed.

How it works

Sizes

Every filter is a sieve. What matters is the size of its holes, in micrometres (µm, thousandths of a millimetre) and nanometres (nm, millionths of a millimetre).

sand grain hair parasite cyst bacterium virus protein salt ion, water 1 mm 100 µm 10 µm 1 µm 0.1 µm 10 nm 1 nm 0.1 nm size, each mark ten times smaller than the last folded cloth sand filter, paper microfilter: fired clay candle ultrafilter: cellophane, hollow fibre nanofilter reverse osmosis: stops nearly all salt each bar shows what that filter stops; anything smaller passes Dead-endCrossflow dirt piles upflow chokes all waterforced through feedconcentratepermeate(clean water) permeate
Fig. 1 The filtration ladder. On the scale, from left to right, things get smaller by ten times at each mark: grains of sand, hairs, parasite cysts, bacteria, viruses, proteins and finally dissolved salt. Under it, the filter that stops each size. Bottom: in dead-end filtration all the water is forced through and the dirt piles up on the membrane; in crossflow, the feed sweeps across the surface and carries the dirt away.
Filter Holes Stops Lets through
Cloth folded 4–8 times 20–100 µm Water fleas, guinea worm, large silt Bacteria, everything smaller
Sand filter, paper 5–20 µm Silt, most parasite cysts Many bacteria
Microfilter (ceramic candle, membrane) 0.1–1 µm Bacteria, cysts, cloudiness Viruses, dissolved things
Ultrafilter 2–100 nm Viruses, proteins, colloids (very fine suspended particles) Sugar, salts
Nanofilter about 1 nm Hardness, colour, larger dissolved molecules Much of the common salt
Reverse osmosis no real holes 95–99.8% of all salt Water, some small gases

A bacterium is 0.5–5 µm long; a virus 20–300 nm. A dissolved sodium ion is about 0.3 nm, barely bigger than a water molecule, so no sieve can tell them apart. Reverse osmosis works another way (below).

Dead-end and crossflow

Pour water through a filter and the dirt piles up on its face until the flow chokes. This is dead-end filtration, fine for small jobs. Crossflow sweeps the feed fast across the membrane, so only part passes through and the rest carries the dirt away, as in every industrial membrane. The water that passes is the permeate; what is left is the concentrate (or brine).

Osmosis

Some films let water through but hold back what is dissolved in it. These are semipermeable membranes: pig bladder, a film of copper ferrocyanide, cellophane and cellulose acetate all behave this way to some degree. Put fresh water on one side and salt water on the other, and water flows by itself into the salty side. This is osmosis. It is why salted meat dries out and drinking sea water kills.

The flow stops when the salty side is pressed hard enough to balance the pull. That pressure is the osmotic pressure: roughly 0.75–0.8 bar for each gram of salt per litre.

Water Salt (g/L) Osmotic pressure
Good drinking water under 0.5 under 0.4 bar
Brackish well 1–10 1–8 bar
Sea water 35 about 27 bar
Brine leaving a seawater plant 60–70 45–55 bar

Reverse osmosis

Press on the salty side harder than its osmotic pressure and the flow reverses: water is squeezed out through the membrane and the salt stays behind. This is reverse osmosis (RO). The film has no holes in the ordinary sense; water dissolves into the polymer and wanders through it far faster than salt can.

The pressure must be well above osmotic, because the brine gets saltier as water leaves it and the extra pressure is what drives the flow: brackish water needs 10–20 bar, sea water 55–70 bar. Only part of the feed comes out fresh, the recovery: 75–85% from brackish water, 35–50% from sea water.

Energy. A modern seawater RO plant uses 3–4 kWh per cubic metre (the theoretical least is about 1 kWh). Boiling the same water once takes about 630 kWh of heat, which is why distillation plants reuse their heat many times over.

What you need

Item Use See
Clay, sawdust or rice husk, a kiln Ceramic filters Pottery, The Kiln
Viscose, acid bath Cellophane film and tube Rayon and Nylon
Cellulose acetate, acetone, formamide Salt-rejecting membranes Ether, Acetone and Solvents, Organic Synthesis and Fine Chemicals
Porous support: fired stoneware, sintered bronze, perforated plate with fine cloth Holding membranes Powder Metallurgy
Plunger pump, gauges, check valves, safety valve 20–70 bar Hydraulic Presses and Rams, Pressure and Vacuum Gauges
Pressure vessel and pipe of stainless steel, bronze or plastic, never plain steel Pressure Vessels and Valves, Petrochemicals and Modern Plastics
Sand filter, activated carbon, conductivity cell Pre-treatment, testing Water Treatment for a Town, Activated Charcoal, Water Softening and Ion Exchange

Where to find it

  • Clay: any good plastic pottery clay; red earthenware clays work well (Finding and Preparing Clay). Sawdust and rice husk burn out and leave the pores.
  • Brackish water: wells in dry plains, coastal aquifers, old sea beds. Water tastes salty at about 0.5 g/L and is undrinkable for most people above 2–3 g/L.
  • Sea water: draw it from a well or a buried pipe in beach sand, not the open surf; the sand filters it.

The ceramic water filter

The simplest membrane, and one of the most useful objects in this book. It needs only a potter.

The pot filter is a flower-pot shape about 30 cm across and 25 cm deep, holding 7–10 litres, of clay mixed with burnable grains, fired porous, and hung in a covered bucket or jar with a tap.

  1. Mix. Powder the clay; sieve sawdust or rice husk through window screen (about 1 mm). Mix roughly equal volumes of clay and sawdust (about 60 : 40 by weight), add water, and knead stiff. Adjust by trial.
  2. Shape in a two-part press mould or on the wheel (The Potter's Wheel): walls and bottom 12–15 mm thick, with a 3 cm rim to hang it by.
  3. Dry slowly in shade for a week or more.
  4. Fire to about 850–900 °C (dull cherry to cherry red) and hold an hour (The Kiln). The sawdust burns out, leaving a sponge of fine, connected pores.
  5. Flow-test. Soak overnight, fill to the brim, and catch what drips through in an hour: 1–2.5 litres is right. Faster means pores too big (less or finer sawdust, or fire hotter); slower is safe but tiresome.
  6. Silver coat (optional). Brush inside and out with weak colloidal silver or silver nitrate (Silver Nitrate and Silver Salts), which kills bacteria caught in the pores and stops slime.
  7. Set it in a glazed pot or bucket with a lid and a low tap. Never touch the outside of the pot with dirty hands.

Such filters remove 99% or more of bacteria. They do not reliably stop viruses: boil or chlorinate as well during an epidemic.

The filter candle is the older factory form: a closed tube of unglazed porcelain, about 25 mm across and 15–25 cm long, walls 4–6 mm, glazed only at the open end where it is cemented into a cap. Use porcelain or kaolin body with finely ground fired grog (crushed fired clay) and no sawdust (Stoneware and Porcelain); slip-cast it (Slip Casting, Jiggering and Ceramic Factories) and fire it to just short of vitrifying (glazing over inside): it should ring when tapped, yet a drop of water on it should soak in within seconds. Hang two or three in the top half of a two-part stoneware jar, the household and hospital "gravity filter" of the 19th century, or fix one to a tap under mains pressure.

Good or bad? Hold the wet filter under water and pump air into it at 0.3–0.5 bar: a steady stream of bubbles marks a crack; discard it. Prove the first filters of each batch with the coliform test (Water Treatment for a Town). When the flow drops, scrub the outside with a stiff brush, never with soap, and boil the filter every few weeks.

The ultrafilter

An ultrafilter stops viruses and protein molecules. It needs a cast film of polymer.

From cellophane. Cellophane is a film of regenerated cellulose, made by squeezing viscose through a slot into an acid bath (Rayon and Nylon). Its pores are a few nanometres: it holds back proteins and anything larger and passes water, salts and sugar. For membranes, make it without glycerine and never let it dry, since drying collapses the pores for good; store it under water with a few drops of formalin (Methanol and Formaldehyde). Clamp a disc of wet film over a porous support (sintered bronze, or fine cloth on a perforated brass plate) between two flanges with a rubber ring (Rubber), fill the space above with liquid, and press it with air at 1–4 bar, stirring above the film so protein does not gel on it. Clear liquid passes, slowly.

This is a laboratory tool for concentrating proteins, cleaning serum and vaccine fluids (Vaccination) and clearing juices. Test it with starch solution: the permeate must give no blue with iodine (Iodine).

Industrial ultrafilters are bundles of thousands of hollow fibres, plastic straws about 1 mm across spun from polysulfone or PVDF, with skins carrying pores of 10–50 nm, potted at both ends in epoxy inside a tube (Resins: Phenolic, Polyester and Epoxy). A module 20 cm across and 1.5 m long holds about 50 m² of fibre and treats 50–100 m³ of river water a day, removing all bacteria and nearly all viruses. Making the fibres needs the Petrochemicals and Modern Plastics industry.

Reverse osmosis

The membrane

Cellulose acetate, cellulose treated with acetic anhydride (Organic Synthesis and Fine Chemicals), is the first workable RO membrane. A dense film of it rejects salt but passes water uselessly slowly. The trick, found in 1960, is to cast an asymmetric film: a skin about 0.2 µm thick on a spongy body 100 µm thick, all in one piece. A recipe that has worked, by weight: 25 cellulose acetate, 45 acetone, 30 formamide, stirred to a clear, thick syrup and left to lose its bubbles.

  1. Spread it on clean glass with a straight bar running on two strips of tape, to a wet thickness of about 0.25 mm.
  2. Let the acetone evaporate from the surface for 30–60 seconds. This forms the skin.
  3. Slide the plate into ice water. The film turns white and floats free. Leave it an hour.
  4. Anneal in water at 70–85 °C for 5–10 minutes. Hotter annealing holds back more salt but passes less water; find the right temperature by trial.
  5. Keep it wet for ever, and mark the skin side: it faces the salt water.

Such films reject 95–98% of salt: plenty for brackish water, but a single pass leaves sea water at about 1 g/L, too salty, so pass it through a second, low-pressure stage. Cellulose acetate wants pH 5–6.5 and below 30 °C; outside that it slowly rots. Bacteria eat it, so keep about 0.5 mg/L of chlorine in the feed.

Polyamide thin-film composite, the modern membrane, rejects 99.5–99.8% at lower pressure. It is a film 0.1–0.2 µm thick formed by reacting two chemicals where they meet, on a porous plastic sheet. It needs an advanced chemical industry, and chlorine destroys it, so its feed must first pass activated carbon.

The element and pressure vessel

  • Flat cell: a disc of membrane, skin up, on a porous support between thick bronze plates, the feed running across it in a 1–2 mm channel. Good for testing.
  • Tubular: membrane cast inside porous tubes 12–25 mm across by drawing a polished bob through them full of syrup, then quenching in ice water. Feed runs down the tube; fresh water seeps out through the wall. Bulky, but easy to clean; the first working plant was tubular.
  • Spiral-wound, the standard: membrane leaves glued into flat envelopes round a coarse permeate spacer, the open edge of each glued along a perforated centre tube, with a plastic net feed spacer about 0.8 mm thick between envelopes, all rolled up and wrapped in glass-fibre and resin.
The unit raw water sand filter 5 µm cartridge plunger pump 15–70 bar gauge safety valve pressure vessel with spiral element feed flows lengthwise along it concentrate valve sets the pressure brine fresh water (permeate) The spiral element, one leaf cut across feed spacer (net) salt water flows here membrane, skin out permeate spacer fresh water flows inward glue seal closes the envelope perforated centre tube fresh water out Many such envelopes, with feed spacer between them, are rolled up round the centre tube.The feed flows along the roll (into the page); fresh water spirals inward to the tube.
Fig. 2 A reverse osmosis unit. Top: raw water passes a sand filter and a 5-micrometre cartridge filter, then a plunger pump raises it to high pressure. Inside the pressure vessel the water flows lengthwise along the spiral element; fresh water passes through the membranes into the centre tube, and the salty concentrate leaves through a valve that holds the pressure. Bottom: one leaf of the spiral element cut across, showing the membrane envelope, the permeate spacer inside it and the feed spacer between envelopes.

A standard element is 20 cm across and 1 m long, holds 35–40 m² of membrane and makes 25–45 m³ of fresh water a day. Up to seven sit end to end in a pressure vessel, a tube of stainless steel or glass-fibre with end caps held by heavy split rings (Pressure Vessels and Valves).

Building a small brackish-water unit

Example: a clinic needs 1 m³ of fresh water a day from a well of 3 g/L.

  1. Membrane area. Cellulose acetate at 15–20 bar passes about 20 litres per square metre per hour: 1,000 ÷ 24 ÷ 20 = about 2 m². Make 2.5 m² to allow for fouling.
  2. Pump. At 50% recovery the feed is 1.4 litres a minute; at 15 bar that is about 35 watts of water power, 50 watts at the shaft, all day and night: about 1.2 kWh. A person on a pedal crank sustains about 75 watts, enough for roughly 60 litres of fresh water an hour, so an hour or two of pedalling morning and evening gives 150–250 litres, the drinking and cooking water of 30–50 people. For the full cubic metre, run it from a small windmill or motor (The Windmill, The Electric Motor). Use a plunger pump: a polished bronze or steel plunger 12–15 mm across in a packed gland, with spring-loaded check valves (Hydraulic Presses and Rams, Packing, Gaskets and Seals).
  3. Pre-treat: settle and sand-filter, then a cartridge of tightly wound cotton yarn stopping particles of 5 µm. A little acid (to pH 6) stops lime scale.
  4. Pressure: a gauge on the pump outlet, a safety valve set 10% above working pressure, and a needle valve on the concentrate line, closed slowly until the gauge reads working pressure. Concentrate and permeate flows should be about equal.
  5. Product: run the first 2 minutes of each start to waste; check with a conductivity cell or by taste.
  6. Brine: to a salt pan (Salt) or far downstream, never back into the well.

Sea water needs four times the pressure, about 280 watts for the same cubic metre: an engine's work, not a person's. Large plants pass the outgoing brine, still at 60 bar, through a pressure exchanger or turbine that hands its energy back to the incoming feed, saving nearly half the power.

Running and cleaning

Log pressures, flows and product saltiness daily. Permeate falling 10–15% at the same pressure and temperature means fouling: clean. Saltier product means a torn membrane, a leaking seal at the centre tube, or a membrane rotted by wrong pH or chlorine. Clean scale with citric acid at pH 2–3 circulated for an hour at low pressure (Citric and Tartaric Acid); clean slime from polyamide with caustic soda at pH 11–12 (Lye and Potash), from cellulose acetate only with mild detergent. Warm water passes about 3% faster per °C, so compare flows at the same temperature.

The solar still

The solar still, a black basin of salt water under sloping glass, is described in Solar Heat. It makes 3–4 litres per square metre per day in strong sun with no fuel. Allow about 1 m² per person for drinking and cooking water, plus a few square metres for cloudy days. The survival still, a plastic sheet over a hole in damp ground, gives well under a litre a day, often less than the sweat spent digging it.

The desalination plant

Where heat is cheap, from a power station or a factory, boiling is still a strong road to fresh water, and it does not care how salty or dirty the feed is.

Multiple effect. Steam boiled off sea water in one closed pan heats the next pan, kept at lower pressure so it boils cooler, and so on; each extra effect makes about as much water again from the same fuel, as in the sugar works (Sugar).

Multistage flash (MSF) is the classic town plant.

stage 1about 105 °C stage 285 °C stage 365 °C stage 440 °C steam in brine heater condensate back to boiler hot brine into stage 1 cold sea water in fresh water out brine out: most recycled, some to sea pressure and temperature fall stage by stage tubes: incoming sea water condenses the vapour, and is warmedtrays under the tubes catch the fresh water
Fig. 3 A multistage flash desalination plant, four stages shown (real plants have 15–25). Cold sea water flows through tubes from the last stage to the first, warming as it condenses the vapour in each chamber, and is brought to about 110 °C in the brine heater by steam. The hot brine then flows back through the chambers, each at lower pressure; in each, part of it flashes into vapour, which condenses on the tubes and drips into a tray as fresh water.
  1. Sea water flows inside banks of tubes running through a row of 15–25 closed chambers, from the coolest to the hottest, gathering heat as it goes.
  2. In the brine heater, low-pressure steam, often exhaust from a The Steam Turbine, brings it to 90–112 °C. Hotter would lay hard scale on the tubes.
  3. The hot brine enters the first chamber, held just below its boiling pressure. Part of it flashes, boiling instantly and cooling itself by 3–5 °C. The vapour condenses on the cool tubes above and drips into a distillate tray.
  4. The brine passes through a slot to the next chamber, at lower pressure, and flashes again. The last sits at 35–40 °C under a vacuum kept by steam jet pumps (The Vacuum Pump).
  5. Only about a tenth of the brine flashes per pass, so most is recirculated, and part is let out to keep it from getting too salty.

A good plant makes 8–10 kg of water per kilogram of heating steam. Use copper-nickel tubes (Nickel and Cobalt) and epoxy-lined or stainless chambers: sea water near boiling eats ordinary steel. Strip air from the feed and dose a little acid or polyphosphate against scale.

After treatment. Distilled and RO water is aggressive: it dissolves pipes and tastes flat. Pass it over crushed limestone or dose lime and carbon dioxide to give it 50–100 mg/L of hardness (Lime), then chlorinate it like any town water.

Dialysis membranes, in outline

Dialysis separates by diffusion, not pressure: small molecules (salts, sugar, urea) wander through a membrane from the stronger side to the weaker; proteins and cells stay behind.

The dialysis bag is a laboratory tool: tie off a length of wet cellophane tube (or sausage casing), fill it with a protein solution, tie the other end leaving room to swell, and hang it in a large jar of pure water changed several times over a day or two. The salt leaves; the protein stays. Bury the bag in dry sugar instead and osmosis draws the water out, concentrating it.

The artificial kidney (Kidney Dialysis) does the same to blood. Blood flows on one side of a large membrane, 1.5–2 m² of hollow fibres in a modern dialyser, and warm, sterile dialysis fluid with the salts of normal blood flows the other way, carrying off urea, potassium and acids. The first machine, in 1943, wound 30–40 m of cellophane sausage tubing round a drum turning in a bath. Dialysis needs drugs to stop clotting (Heparin and Anticoagulants), hundreds of litres of RO-purified water per treatment, and lasting access to a blood vessel: the work of an established hospital that has mastered Intravenous Fluids and Blood Typing and Transfusion.

How to tell it worked

  • Ceramic filter: 1–2.5 L/h; no stream of bubbles under water at 0.3–0.5 bar; the water grows no coliforms.
  • Ultrafilter: sparkling clear permeate, no blue with starch and iodine.
  • RO: product tastes fresh, with conductivity under one tenth of the feed's.
  • Distillate: tastes of nothing and leaves no ring when dried on clean glass.

Note Troubleshooting. Ceramic filter cracks in firing → dry slower; add fired grog; heat slowly through 100–600 °C. Cast membrane passes salt freely → skin facing the wrong way; bubbles or dust in the syrup; annealed too cool; film once dried out. Cast membrane passes almost no water → evaporated too long or annealed too hot. Output falls week by week → fouling: better pre-treatment, clean on schedule. Salt in MSF distillate → brine carried over by foaming or overfull chambers, or leaking tubes.

Dangers

Danger High pressure. A seawater unit runs at 60–70 bar. A failed hose whips and can inject water through skin, and pressure vessel end caps have blown out and killed when their retaining rings were not seated. Fit a safety valve, guard hoses, never stand at the end of a vessel under pressure, and test every new vessel with water at 1.5 times working pressure.

  • Clean-looking water is not always safe. A cracked filter passes germs unseen. Test filters regularly; boil or chlorinate when in doubt.
  • Chemicals. Acetone burns fiercely: cast membranes outdoors, away from flame (Ether, Acetone and Solvents). Formamide harms unborn children: wear gloves, and keep pregnant women away from it.
  • Brine spilled on fields kills the soil for years. Return it to the sea well away from the intake, or dry it for salt.

What this unlocks

Ceramic filters give safe water to every household without fuel. RO and MSF make towns and farms possible on dry coasts and islands, and supply boilers (Boilers and Pressure Vessels) and Making Microchips. Ultrafiltration gives clean vaccines, serum and river water; dialysis keeps people with failed kidneys alive. Related membranes separate gases (Liquid Air, Nitrogen and the Noble Gases), concentrate milk and juice without heat (Dairy and Cheese), and carry ions inside fuel cells and batteries (Fuel Cells, Storing Energy).

How it was first done

In 1748 the French cleric Jean-Antoine Nollet filled a pig's bladder with alcohol, sank it in water and watched it swell until it burst: the first recorded osmosis. Thomas Graham separated colloids from salts through parchment in 1861 and named it dialysis. Charles Chamberland, working with Louis Pasteur, made the porcelain filter candle in 1884; viruses were discovered in the 1890s as germs that passed through it. Willem Kolff built his drum artificial kidney in the occupied Netherlands in 1943 and saved his first patient in 1945. In 1960 Sidney Loeb and Srinivasa Sourirajan at the University of California, Los Angeles, cast the first asymmetric cellulose acetate membrane, and in 1965 Loeb's tubular plant at Coalinga, California, supplied the town from a brackish well. John Cadotte made the polyamide membrane in the late 1970s. Multistage flash distillation was developed in the 1950s, largely by Robert Silver at the Weir company of Glasgow, and the Gulf states built it on a vast scale. The clay pot filter was designed by Fernando Mazariegos in Guatemala in 1981 and spread worldwide by the group Potters for Peace.