The grey powder that sets hard as stone in an hour and under water. Made by burning finely ground limestone and clay together until they partly melt into clinker at about 1,450 °C, then grinding it with a little gypsum. Hard to do on a small scale — but there is an easier "natural cement" on the way.

Difficulty
●●●●●
Time
Weeks to find and test raw materials; a few days per burn; a day or two of grinding per hundred kilograms by hand
Steps from zero
4 prerequisites →

You need first

LimeThe KilnFinding and Preparing Clay

This unlocks

Reinforced ConcreteBall Mills, Crushers and Grinders
The full path from nothing — 4 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. The Kiln
  4. Lime
  5. Portland Cement

Do them roughly in this order. See it on the tech tree →

Why it matters

Lime mortar sets slowly and only in air; lime and volcanic ash set under water but take weeks (see Mortar and Concrete). Portland cement sets in hours, under water or in air, and becomes several times stronger than any lime: good concrete made with it can carry 20–40 megapascals (MPa) — a column of it the size of a hand can hold up a loaded truck. With it you can build harbours, dams (Dams and Reservoirs), bridges, water pipes, sewers, tall buildings, and, with steel bars inside, Reinforced Concrete.

It is also one of the hardest things in this part to make. It needs:

  • raw materials mixed in the right proportions, ground very fine;
  • a kiln that reaches about 1,450 °C — yellow-white heat, hotter than iron smelting in a bloomery;
  • heavy grinding of a very hard product.

This chapter is honest about that. It gives you three steps, each useful on its own: (1) hydraulic lime (already in Mortar and Concrete), (2) natural cement, which is burned at only 900–1,100 °C, and (3) true portland cement.

How it works

Limestone is mostly calcium carbonate. Clay is mostly silica (silicon oxide), alumina (aluminium oxide) and some iron oxide.

  1. Below 900 °C, the clay loses its water and the limestone begins to lose carbon dioxide, becoming lime (see Lime).
  2. From about 900 to 1,250 °C, lime reacts with the clay's silica, alumina and iron in the solid state, forming belite (a calcium silicate with two parts lime to one of silica). This is the main ingredient of natural cement and hydraulic lime: it hardens with water, but slowly.
  3. At about 1,300–1,450 °C, part of the mix (about a quarter) melts into a liquid. In that liquid, belite takes up more lime and becomes alite (three parts lime to one of silica). Alite is what gives portland cement its fast, high strength. The mass forms hard, dark, partly glassy lumps called clinker, typically 1–3 cm across.
  4. Cooling quickly keeps the alite from changing back.
  5. Grinding the clinker to a flour-fine powder exposes its surface to water.
  6. Gypsum (3–5%) is ground in with the clinker. Without it, the aluminium compounds react with water in seconds and the paste goes stiff almost instantly ("flash set"). Gypsum slows them down so you have an hour or more to work. See Gypsum and Plaster of Paris.

Setting. When cement meets water, the calcium silicates dissolve a little and grow interlocking needles and a gel of calcium silicate hydrate, which binds the sand and stone. This is a reaction with water, not air — so cement sets under water, in a wall's core, or in a sealed mould. It stiffens in 1–3 hours, hardens in a day, and reaches most of its strength in 28 days, gaining more for years.

1. Raw materials3 parts limestone or chalkto 1 part clay, by dry weight 2. Grind and mix wetstir to a cream, sieve,settle, dry to stiff dough 3. Form balls3–5 cm; dry themcompletely 4. Burn to clinker1,400–1,450 °C, white heat,then cool quickly in air 5. Grind with gypsumabout 4 kg per 100 kg clinker,ground flour-fine 6. Cementstore dry and sealed;use within a few months blast clinkergypsum
Fig. 1 From quarry to bag. Limestone and clay are ground together into a raw meal, formed into balls, burned to clinker, cooled, and ground with a little gypsum.

What you need

Item Notes
Limestone or chalk Pure, fizzes strongly; about 3 parts by weight
Clay or shale About 1 part by weight; or a natural marl (clayey limestone) that already has both
Gypsum 3–5% of the clinker weight; see Gypsum and Plaster of Paris
Fuel Charcoal (see Charcoal) or coke (Coal and Coke); roughly 1 kg for every 2–3 kg of raw balls in a small kiln
Grinding Quern stones, an edge-runner mill or millstones (The Watermill); for wet mixing, a tub and paddle
Sieves A fine cloth or woven-hair sieve (openings about 0.1–0.2 mm)
Kiln For natural cement: a lime kiln (Lime). For portland: a firebrick-lined shaft kiln with a forced blast (Firebrick and Refractories, Bellows)
Testing Small moulds, a needle, a pot for boiling, a balance (Measurement from Scratch)

Where to find it

  • Limestone and chalk — see Lime and Rocks and Minerals. Chalk is ideal: soft, pure and easy to grind.
  • Clay and shale — see Finding and Preparing Clay. Any ordinary clay or soft shale. Avoid very sandy clay (coarse quartz grains do not react) and clay with a lot of salt.
  • Marl and "cement rock" — a grey, blue-grey or buff limestone that fizzes in acid but leaves a muddy residue. It is common in thin beds between shales, in lake deposits, and in hard nodules (called septaria) in clays along coasts. Dissolve a weighed chip (about 10 g, crushed) in strong vinegar or acid until fizzing stops, wash and dry the muddy residue, and weigh it. 25–35% residue means a natural cement rock; about 20–25% is close to a portland mix already.
  • Gypsum — soft white mineral that does not fizz; see Gypsum and Plaster of Paris.

Method 1: Natural cement (the achievable first step)

Natural cement is what built canals, aqueducts and the first concrete bridges of the early 1800s. It needs only a lime kiln.

  1. Find cement rock or marl with 25–35% clay (test above). Or make a mix: 2 parts limestone to 1 part clay by dry weight, ground and mixed wet (as in Method 2, steps 1–3), formed into balls and dried.
  2. Burn it in a lime kiln (Lime) broken into pieces 3–6 cm across, at bright cherry to orange heat (900–1,100 °C) for 8–24 hours. Do not go hotter: natural cement rock that is overburnt fuses and becomes useless.
  3. It will not slake. Unlike lime, properly burned natural cement does not hiss and fall to powder when wetted. That is how you know it has become cement and not lime. Lumps that do slake were too pure in lime or underburnt — sort them out.
  4. Grind it to a fine powder (see "Grinding" below). It is much softer than portland clinker.
  5. Use it as you would cement: 1 natural cement : 1–2 sand, mixed with water and used at once — it sets in 15–60 minutes. Keep it damp for a week.

Natural cement is weaker than portland (perhaps a third to half the strength), but it sets fast, sets under water, and is very good for mortar, renders, drains, cisterns and foundations.

Method 2: Portland cement

Step 1: Proportion the raw mix

Real portland clinker is about two-thirds lime (calcium oxide) and one-third clay oxides. That works out at roughly:

3 parts pure limestone or chalk : 1 part clay, by dry weight.

With purer clay (more silica) use a little more limestone (up to 3½ : 1); with a marl that already contains clay, add less clay. Because every rock and clay differs, you must find your own best mix by testing — make several small batches at different ratios (for example 2.5 : 1, 3 : 1, 3.5 : 1), burn them together, and see which gives sound, strong cement (tests below). Write everything down.

  • Too much limestone → free lime left in the clinker, which slakes and swells weeks later and cracks the concrete (unsound).
  • Too much clay → weaker, slower cement (more belite), and the clinker melts and sticks to the kiln too easily.

Step 2: Grind and mix very fine

The reactions happen where tiny grains of lime and clay touch, so the raw mix must be intimately mixed and flour-fine. Coarse grains of limestone come out as free lime; coarse quartz grains do not react at all.

  1. Wet method (best for chalk and soft clay). Put chalk and clay, weighed, into a tub or a lined pit with plenty of water and stir hard with paddles (or with a horse-driven harrow in a ring-shaped trough — a wash mill). Both break down into a thin cream.
  2. Sieve the slurry through fine cloth, letting grit and stones stay behind.
  3. Settle and dry. Let it settle in shallow pits for a few days, pour off the clear water, and let the paste dry to stiff dough — on a floor warmed by the kiln's waste heat if you can.
  4. Dry method (for hard limestone). Crush and grind limestone and clay separately to fine powder in a quern, weigh, mix thoroughly, and dampen.
  5. Form balls or bricks. Roll the stiff paste into balls 3–5 cm across (or cut it into small bricks) and dry them fully in the sun or near the kiln. They must be bone dry before burning or they will burst.

Step 3: Burn to clinker

You need yellow to white heat — about 1,400–1,450 °C (see the glow colours in The Kiln) held long enough for the mix to sinter (partly melt and fuse). This is past the limit of an ordinary wood-fired pottery kiln (see Very-High-Temperature Furnaces; Pyrometric Cones and Kiln Temperature tell you when you have reached it). Historically, small works used tall bottle kilns or shaft kilns filled with layers of coke and raw balls. On a small scale:

Hot gases outcarbon monoxide burns blue Charge in layers8–10 cm charcoal, 8–10 cm raw balls;balls dry and heat as they sink Stone or brick wall 900–1,250 °Clime forms and starts to combinewith the clay Burning zone 1,400–1,450 °Cwhite, too bright to look at:the mix partly melts into clinker Draw holetake out cooled clinker every 1–2 hours Firebrick liningordinary clay melts here Tuyeresblast from bellows,30–40 cm above floor 1.5–2.5 mtall 40–60 cm inside
Fig. 2 A small shaft kiln for cement clinker, in section. Raw balls and charcoal go in at the top in alternating layers. A blast from bellows makes a white-hot burning zone low in the shaft; clinker sinks through it, cools, and is drawn out at the bottom.
  1. Build the kiln. A round shaft 40–60 cm inside and 1.5–2.5 m tall, of stone or brick, lined with firebrick or fireclay mixed with grog (Firebrick and Refractories). Ordinary clay melts at these temperatures. Leave two or three tuyeres (clay air pipes) about 30–40 cm above the floor, and a draw hole at the bottom closed with a firebrick door.
  2. Preheat with wood, then fill the lower part with charcoal and start the blast from Bellows (or a water-powered blower; see The Waterwheel).
  3. Charge in layers: a layer of charcoal 8–10 cm thick, then a layer of raw balls 8–10 cm, and so on to the top. Start with 1 part charcoal to 2 parts raw balls by weight, and adjust.
  4. Blow hard and steadily. The zone in front of the tuyeres should be white, too bright to look at. Balls slowly sink through it as fuel burns away.
  5. Draw clinker from the bottom every hour or two, once the lowest balls have passed through the hot zone and cooled a little, and add fresh layers on top. Spread drawn clinker out on stone to cool quickly in the air.
  6. Watch for sticking. If the charge hangs (stops sinking) or the clinker fuses into large glassy masses stuck to the wall, the kiln is too hot or the mix has too much clay. Poke it down with an iron bar through the top or the tuyeres.

Step 4: Grinding

Clinker is very hard. Grinding is the hardest work in cement making.

  1. Crush clinker on an anvil stone with a hammer to pea size.
  2. Add gypsum: about 4 kg raw gypsum for every 100 kg of clinker.
  3. Grind them together. Use a hard stone quern (Grain, Flour and Bread), or better, an edge-runner: a heavy stone wheel rolling round a stone trough, turned by an animal (Draft Animals and Harness) or water. A ball mill — a wooden or iron drum half full of hard flint pebbles, turned slowly on its axis — grinds very fine with little attention (The Watermill, Ball Mills, Crushers and Grinders).
  4. Sieve through the finest cloth you have. The powder should feel like flour, not sand, when rubbed between finger and thumb, and at least 85–90% should pass the sieve. Regrind what stays behind.
  5. Store dry in sealed pots or barrels (Barrels and Cooperage). Cement soaks up damp from the air and sets in lumps; use it within a few months.

How to tell it worked

The clinker

Looks like Means
Dark grey-green to greenish-black, hard, heavy lumps with a slightly glassy, sintered surface; does not slake or get hot in water Good clinker
Yellowish or buff, light, soft, crumbles; slakes and gets hot in water Underburnt — lime and belite only; reburn or use as hydraulic lime
Black, shiny, glassy slag fused to the kiln wall Overburnt or too much clay — use less fuel or more limestone
Mostly good, but with white spots Coarse limestone grains or poor mixing — grind the raw mix finer

The cement

  1. Set test. Mix 100 g cement with 25–30 g water into a stiff paste and pat it into a pat 1 cm thick. Make a "needle": a nail about 1 mm thick, fixed in a stick weighted to about 300 g. Every 15 minutes lower the needle gently onto the paste. It should start to stiffen (the needle stops going right through) after 45 minutes to 3 hours, and be hard (the needle leaves barely a mark) within 10 hours. Setting in a few minutes means it needs more gypsum; not setting overnight means underburnt or bad clinker.
  2. Soundness (the boiling test). Make two pats about 8 cm across and 1 cm thick on flat glass or glazed tile; keep them under a damp cloth for 24 hours, then boil them in water for 3 hours. Sound cement comes out whole. If the pat cracks round its edges, bends, or crumbles, there is free lime in it — use more clay or finer grinding, and do not use this batch for structures.
  3. Strength — the bar test. Mix 1 part cement to 3 parts clean sand with half the cement's weight in water. Pack it into wooden moulds 4 × 4 × 16 cm, cover with a damp cloth for a day, then cure the bars under water for 7 and 28 days. Rest each bar on two supports 10 cm apart and hang a basket of stones from the middle until it breaks. A good portland cement bar at 28 days takes roughly 150–300 kg (use a lever, see Simple Machines, to multiply a smaller weight). Natural cement and hydraulic lime take far less. Compare batches side by side — that is how you improve.
  4. Underwater pat. A pat put straight into water an hour after mixing should set hard there within a day.

Note Troubleshooting. Clinker yellowish and slakes → not hot enough or not long enough in the hot zone; stronger blast, more charcoal, slower drawing. Kiln charge fuses into one mass → too hot, or mix too rich in clay or iron; increase limestone a little, reduce fuel, and keep balls small and dry. Cement sets in a few minutes ("flash set") → not enough gypsum, or gypsum was overheated in grinding; add a little more raw gypsum. Pats crack in the boiling test → free lime; reduce limestone, grind the raw mix finer, burn hotter. Weak bars → grind the cement finer (this matters more than anything else you can do quickly), check the sand is clean, and cure the bars wet. Cement gone lumpy in store → damp got in; sieve out lumps and use the rest for less important work.

Using cement

  • Mortar: 1 cement : 3–4 sand. Add 1 part lime putty for a mortar that is easier to work and less brittle (1 : 1 : 6 cement : lime : sand is a good general wall mortar).
  • Concrete: 1 cement : 2 sand : 4 gravel (up to 2–3 cm) by volume, a common general-purpose mix. For water-tight tanks, 1 : 1½ : 3.
  • Water: use the least water that lets you work it: about half the weight of the cement. Extra water makes concrete weaker and more porous — a sloppy mix can lose half its strength.
  • Mix dry until the colour is even, then add water and mix again; place within an hour; tamp or rod it to drive out air.
  • Cure damp for at least 7 days, shaded, frost-free. Concrete that dries out early never reaches its strength.

For walls, floors, slabs and beams, continue in Reinforced Concrete and Foundations and Floors.

Dangers

Danger Cement burns. Wet cement is very alkaline (as strong as Lye and Potash). Kneeling in fresh concrete or letting it run into boots causes deep, painful burns that may not be felt for hours. A splash in the eye can blind — flush with clean water for at least 20 minutes at once. Wear gloves or wrapped hands and cover knees and legs; wash skin promptly.

Danger The kiln. A cement kiln is hotter than a bloomery, and makes carbon monoxide in quantity. Burn only in the open, never sleep near it, and never climb onto or into a kiln, even a cooling one. White-hot clinker and fused slag can burst when they touch water — keep the drawing area dry. Protect your eyes from the white glow with a dark leather or smoked-glass shield and do not stare into it.

  • Dust. Raw meal, clinker and cement dust irritate the lungs and eyes and contain fine silica. Grind wet where possible, cover the mill, and wear a damp cloth over nose and mouth.
  • Free lime. Cement that failed the boiling test can crack a structure months later. Test every batch before using it for anything that carries a load or holds people.

What this unlocks

Portland cement makes concrete for Foundations and Floors, dams, harbour walls, Wells and Cisterns, pipes and Sewers and Wastewater, Roads and Bridges, and the cast concrete of Reinforced Concrete buildings. It enabled the great water and sanitation works that made cities healthy (Sanitation and Germs).

How it was first done

In 1756 John Smeaton showed that limestones containing clay make lime that sets under water. In 1796 James Parker patented "Roman cement", burned from clay-rich limestone nodules found on the Thames estuary — a natural cement. In France, Louis Vicat worked out in 1817–1818 how to make artificial hydraulic lime by burning lime and clay together. In 1824 Joseph Aspdin, a bricklayer in Leeds, patented "Portland cement", named for its likeness to the pale building stone of Portland in Dorset, though his product was probably burned too cool to be true modern cement. In the 1840s, Aspdin's son William and Isaac Charles Johnson in England found that burning the mix much hotter, until it partly fused into clinker, gave a far stronger cement — the first true portland cement. Early cement was burned in bottle and shaft kilns with coke and ground in millstones. The rotary kiln — a long, slowly turning, inclined steel tube — was developed in England and the United States in the 1880s and 1890s and made cement cheap enough to build the modern world.

Source: content/entries/earth/portland-cement.md