◆ Rebuild

Part 8 · Chemistry

Silicones and Synthetic Rubbers

Natural rubber goes sticky in heat, cracks in sunlight and swells in oil. Silicones — chains of silicon and oxygen made from sand, wood spirit and salt — give oils whose thickness hardly changes from frost to oven heat, greases for taps and glass joints, and rubbers that stay soft from −55 to +230 °C. Neoprene and nitrile rubbers, built from acetylene, alcohol or oil, stand up to weather and to petrol. This chapter gives their making in outline, and in full how to choose, design, mould and test the O-rings and seals that use them.

Difficulty
●●●●●
Time
An afternoon to make a grease or a sealant from bought-in or works-made silicone; a day to make an O-ring mould on the lathe and mould the first rings; a silicone or synthetic rubber works is a national project
Steps from zero
43 prerequisites →

You need first

Pure SiliconRubberOrganic Synthesis and Fine Chemicals

This unlocks

Synthetic Rubber Works (Overview)
The full path from nothing — 43 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Simple Machines
  8. Hunting and Trapping
  9. Basic Woodworking
  10. Charcoal
  11. Pottery
  12. The Kiln
  13. Quarrying and Cutting Stone
  14. Rubber
  15. Hides and Leather
  16. Bricks
  17. Lime
  18. Salt
  19. Mining and Tunnelling
  20. Lye and Potash
  21. Fermentation
  22. The Wheel and Axle
  23. Firebrick and Refractories
  24. Glass
  25. Bellows
  26. Saltpeter
  27. Distillation
  28. Gears
  29. Coal and Coke
  30. Iron (the Bloomery)
  31. Copper Smelting
  32. Sulfuric Acid
  33. Coal Tar Chemicals
  34. Laboratory Glassware
  35. The Waterwheel
  36. Blacksmithing
  37. Hydrochloric Acid
  38. Organic Synthesis and Fine Chemicals
  39. Magnets
  40. Copper Wire
  41. The Generator
  42. The Electric Arc Furnace
  43. Pure Silicon
  44. Silicones and Synthetic Rubbers

Do them roughly in this order. See it on the tech tree →

Why it matters

Packing, Gaskets and Seals covers hemp, leather, gaskets and a first O-ring, and Rubber the rubber itself. But natural rubber goes soft and sticky above about 80 °C, swells to jelly in oil and petrol, and cracks in sunlight and ozone (the sharp-smelling gas made by sparks).

Silicones solve heat. Their backbone is silicon and oxygen, the atoms of quartz, so they shrug off heat, frost, water and sunlight: oils for instruments and baths, greases for glass taps (Laboratory Glassware), rubbers for oven doors, sterilisers (Sterilising Instruments and Dressings) and medical tubing, and sealants for windows. Synthetic rubbers solve oil and weather: nitrile seals oil, fuel and hydraulics (Hydraulic Presses and Rams, The Internal Combustion Engine); neoprene resists weather and fire.

All need a real chemical industry, so their making is given in outline. What a workshop can do — compound, mould, cure and test seals, above all the O-ring — is given in full.

How it works

Rubber is tangled chains, tied together. Long, flexible chain molecules form a tangle that stretches and springs back. Untied, the chains slide past each other and the lump slowly flows; tied here and there (curing, as sulfur does for natural rubber), it becomes a true rubber.

Silicones have a backbone of silicon and oxygen atoms in turn, with two methyl groups (carbon with three hydrogens) on each silicon. The silicon–oxygen link survives heat that breaks carbon chains; the chain stays limber far below freezing; and the methyl coat sheds water. Short chains are an oil, long chains a gum that cures to rubber, and branched chains hard heat-proof resins.

Synthetic rubbers are carbon chains built from chosen building blocks. A chlorine atom on the chain (neoprene) resists weather and fire; nitrile groups (carbon triple-bonded to nitrogen) keep oil out.

Rubber Range, °C Good with Bad with
Natural rubber −50 to +80 Water, air, mild acids; strongest and springiest Oil, petrol, sunlight, ozone, heat
Nitrile (NBR) −30 to +110 Mineral oil, petrol, diesel, grease, water Sunlight and ozone, brake fluid, acetone
Neoprene (chloroprene) −35 to +110 Weather, ozone, seawater, refrigerant gas; self-extinguishing Petrol, strong oxidisers
Silicone −55 to +230 Dry heat, cold, sunlight, food and body contact Petrol and oil (swells), tearing, rubbing, high-pressure steam; leaks gas in vacuum
EPDM −45 to +140 Steam, hot water, brake fluid, weather Any oil or petrol
Butyl −40 to +120 Gas-tight: inner tubes, gas bags Oil
Fluoroelastomer −20 to +200 Hot oil, fuel, acids, vacuum Cost; needs fluorine chemistry (Fluorspar and Fluorine Compounds)

What you need

Item Use See
Silicon, metallurgical grade, crushed Silicones Pure Silicon
Methanol (wood spirit) and hydrogen chloride Methyl chloride Ether, Acetone and Solvents, Hydrochloric Acid
Copper powder Catalyst Copper Smelting
Distillation column, tall, with reflux Separating chlorosilanes Distillation
Fine silica: fumed or precipitated Thickening grease, reinforcing rubber Below, Water Glass (Sodium Silicate)
Peroxide curing agent Silicone rubber Hydrogen Peroxide and Oxygen Bleach, Organic Synthesis and Fine Chemicals
Two-roll mill, lathe, steel plate, dowel pins Mixing rubber; O-ring moulds Rubber, The Lathe
Heated press, 150–180 °C Moulding Hydraulic Presses and Rams, Presses, Punches and Dies
Vernier calliper Checking Rules, Squares, Callipers and Gauges

Where to find it

The raw materials are ordinary: quartz sand or vein quartz and charcoal for silicon (Pure Silicon); hardwood for the wood spirit of methanol (Charcoal, Ether, Acetone and Solvents); salt for hydrogen chloride (Salt, Hydrochloric Acid); copper (Copper Smelting). Synthetic rubbers start from carbide acetylene (Calcium Carbide and Acetylene), from alcohol fermented from grain or sugar (Fermentation), or from crude oil cracked to gases (Petroleum and Refining, Petrochemicals and Modern Plastics).

Making silicones (in outline)

Silicon powder quartz + charcoal, arc Methyl chloride wood spirit + HCl Direct process copper, 280–300 °C Hydrolysis into cooled water Oil or gum chains grown, 150 °C Grease + fine silica Rubber + silica, peroxide Sealant + cross-linker Column, 100+ plates Trimethylchlorosilane, 57 °C a few % : caps chain ends Methyltrichlorosilane, 66 °C 5–15 % : resins, sealant cross-linker Dimethyldichlorosilane, 70 °C 80–90 % : makes the chains vapour hydrogen chloride goes back cooled: above 320 °C it runs away
Fig. 1 From sand to silicone. Silicon from the arc furnace and methyl chloride from wood spirit and hydrogen chloride meet over a copper catalyst at 280–300 °C. A tall column separates the liquid chlorosilanes. The main one, dimethyldichlorosilane, is stirred with water to make silicone chains and hydrogen chloride, which goes back to make more methyl chloride. The chains become oil, gum, grease, rubber and sealant.
  1. Methyl chloride. Methanol vapour and dry hydrogen chloride over alumina at about 300–350 °C. It is a gas boiling at −24 °C, stored as a liquid under pressure (Pressure Vessels and Valves).
  2. The direct process. Silicon powder (about 0.05–0.3 mm) mixed with 5–10 % copper and a trace of zinc, in a stirred or fluidised steel reactor at 280–300 °C, with methyl chloride blown through. The silicon turns into liquid methylchlorosilanes, condensed from the off-gas. The reaction makes heat; above about 320 °C it runs away to soot and the wrong products, so the reactor is cooled.
  3. Separate. About 80–90 % is dimethyldichlorosilane (boils at 70 °C), which makes chains; 5–15 % methyltrichlorosilane (66 °C), which makes branches; a few percent trimethylchlorosilane (57 °C), which caps chain ends. The first two boil 4 °C apart, so the column needs well over a hundred plates, tens of metres tall (Distillation).
  4. Hydrolyse. Dimethyldichlorosilane run into stirred, cooled water gives silicone oil and hydrogen chloride, which goes back to step 1: the chlorine goes round in a circle.
  5. Grow the chains by heating at about 150 °C with a trace of caustic potash. The end-cap (from trimethylchlorosilane) sets chain length: more cap, thinner oil; almost none, a gum. Strip off volatile rings at 150–200 °C under vacuum (The Vacuum Pump).

Kipping's older laboratory route uses silicon tetrachloride (Pure Silicon) with a Grignard reagent made from Magnesium and methyl chloride in dry ether (Organic Synthesis and Fine Chemicals).

Silicone oil

Clear, colourless and nearly odourless, graded by thickness in centistokes: water 1, sewing machine oil about 30, castor oil about 1,000, honey about 10,000. It thins only about 2.5 times between 40 and 100 °C, where a mineral oil thins about 9 times; it pours at −50 °C and thick grades will not burn below about 300 °C. To grade it, time a ball bearing falling 10 cm through it in a glass tube against oils of known grade.

Uses: damping fluid in meters and compasses (Measuring Electricity, The Compass); heating baths to 250 °C (Burners, Stands and Laboratory Equipment); mould release (Metal Casting); gas chromatograph columns (Chromatography); a few drops per 100 litres kill foam in fermenters (Fermentation).

Silicone grease

Silicone grease is silicone oil thickened with very fine silica, so it stays a soft paste from −40 to +200 °C.

The silica. Best is fumed silica: silicon tetrachloride (Pure Silicon) burned in a hydrogen–oxygen flame gives a white smoke of particles so fine that a litre weighs 50 g. Second best is precipitated silica: acid stirred into dilute water glass (Water Glass (Sodium Silicate)), washed free of salt, dried and ground.

Making it.

  1. Put 100 g of silicone oil of 1,000–10,000 centistokes in a glazed mortar or on a slab.
  2. Work in 6–10 g of fumed silica (or about twice as much precipitated silica) a pinch at a time, grinding each in before the next, until it stands in peaks like petroleum jelly. More silica, stiffer grease.
  3. Pass it two or three times between steel rollers set almost touching, or grind longer, until there are no lumps.
  4. Remove air bubbles by standing the jar in a vacuum chamber for an hour (The Vacuum Pump). Pack in tubes or tins.

Uses: glass taps and joints; nitrile and natural rubber O-rings on assembly; electrical connectors and ignition leads (Insulators, Cables and Electrical Fittings); valves in food machinery.

A good grease is smooth and translucent with no grit; a blob stays put on a 200 °C hot plate; on blotting paper it leaves only a narrow ring of oil after a day. Lumpy means the silica was not worked in; runny or bleeding means too little silica.

Warning Silicone grease spoils surfaces. A trace creeps over metal and glass, and paint, glue, solder and plating will not stick there afterwards. Keep it away from anything to be painted, and use the least you can. In high-vacuum systems prefer the greases in High-Vacuum Pumps and Gauges. Never grease silicone rubber with it: silicone oil swells silicone rubber.

Silicone rubber and seals

Compounding (heat-cured rubber). On a cold two-roll mill (Rubber), band 100 parts of silicone gum and work in:

Ingredient Parts Why
Fumed silica 25–40 Without it silicone rubber is weak as cheese; with it, strong
Short, water-ended silicone oil 3–8 Keeps the stock from stiffening on the shelf
Red iron oxide 0–2 Improves heat resistance; gives the classic brick-red colour
Peroxide, e.g. dicumyl peroxide 0.5–1.5 The curing agent. Add it last, cold

Moulding and curing. Press in a heated mould (see O-rings below) at 165–175 °C for 5–10 minutes, then post-cure in a vented oven at 200 °C for 4 hours. Without post-cure the seal smells, stays tacky and takes a permanent set.

Silicone rubber seals made this way: pressure cooker and kettle rings, oven and steriliser door seals, lamp gaskets, teats and tubing (Stretchers, Hospital Beds and Patient Equipment). Long hollow door seals are pushed through an extruder die (Petrochemicals and Modern Plastics) and cured in a hot-air tunnel at 200–300 °C. A good seal is evenly coloured, stretches to twice its length and recovers, and springs nearly back after a day squeezed in a 200 °C oven. Silicone tears easily: avoid sharp corners in the design.

Silicone sealant and mould rubber (RTV). "Room-temperature vulcanising" silicones cure without heat:

  • Sealant: silicone oil with water-reactive ends, 8–12 % fumed silica and 4–6 % of a cross-linker made from methyltrichlorosilane and acetic acid, filled airless into tubes. Damp air cures it from the skin inward, 2–3 mm a day, smelling of vinegar. For glazing, bathrooms and gasket-in-place joints.
  • Mould rubber: the same oil and filler, with 2–5 % ethyl silicate (silicon tetrachloride and alcohol) and 0.5–1 % tin catalyst stirred in just before pouring. It sets in a day and copies a fingerprint, for casting plaster, wax and resin (Slip Casting, Jiggering and Ceramic Factories).

Neoprene and nitrile (in outline)

Both are made as a synthetic latex: the building blocks are stirred into soapy water and joined into chains by a persulfate starter, stopped at about 70 %, stripped of leftover gas with steam, then curdled with salt and acid, washed and dried. This needs gas-tight pressure reactors and refrigeration; the works, and the SBR, butyl and EPDM made alongside, are described in Synthetic Rubber Works (Overview).

Neoprene comes from acetylene (Calcium Carbide and Acetylene): over a copper(I) chloride catalyst it pairs into vinylacetylene, which with hydrogen chloride gives chloroprene (boils at 59 °C), polymerised at about 40 °C. It cures with 4 parts magnesium oxide and 5 zinc oxide per 100 at 150–160 °C. Dissolved in solvent it is the best contact adhesive for leather and shoe soles (Glues and Adhesives, Footwear).

Nitrile is butadiene and acrylonitrile polymerised together at 5–10 °C. Butadiene comes from cracked oil gases or, as in the Soviet Union from 1932, from alcohol vapour over a magnesia–silica catalyst at about 400 °C; acrylonitrile from propylene, ammonia and air in a petrochemical works. About a third acrylonitrile is the usual grade; more resists oil better but stiffens in cold. It cures like natural rubber: per 100 parts, 1.5 sulfur, 1–2 accelerator, 5 zinc oxide, 1 stearic acid, 40–70 carbon black, at 150–170 °C (Lampblack and Carbon Black).

O-rings

The O-ring is the most useful seal ever made: a ring of round section, squeezed in a rectangular groove. With no pressure, the squeeze alone seals it. Under pressure, the fluid pushes the ring across the groove into the far corner, and the harder it pushes, the harder the ring seals. One O-ring can hold anything from a hard vacuum to several hundred bar.

1. Free in the groove 2. Closed: squeezed 3. Under pressure Width 1.3–1.5 × cord depth 0.72–0.80 × cord (static) ring stands proud of the face Squeezed 20–30 % (10–20 % for moving seals) fills at most 85 % of the groove Pushed into the far corner the harder the push, the tighter pressure Gap under 0.1 mm or rubber is nibbled out Standard cord thicknesses in millimetres, drawn to the same scale 1.782.623.535.336.99
Fig. 2 The O-ring and its groove. A ring of round section sits in a rectangular groove; when the parts close it is squeezed by about a quarter. Pressure pushes it into the corner away from the fluid, where it seals harder. The gap between the parts must be small or the rubber is forced into it and nibbled away. The standard cord thicknesses are 1.78, 2.62, 3.53, 5.33 and 6.99 mm.

Choosing the rubber

Service Use Never
Water, air, up to 80 °C Natural rubber or nitrile —
Mineral oil, hydraulics, petrol, diesel Nitrile Natural, silicone, EPDM
Brake fluid, steam, hot water above 100 °C EPDM Nitrile, natural
Dry heat to 200 °C, food, medicine Silicone Moving seals, oil
Weather, refrigerant gas, seawater Neoprene Petrol
Vacuum Nitrile, or fluoroelastomer if baked Silicone (gas soaks through)

Standard hardness is 70 on the Shore A scale. As a thumb guide: a rubber band is about 30, a pencil eraser about 50, a car tyre tread about 65–70, a shoe heel about 80. Use 90 for pressures above about 100 bar or for large gaps.

Sizes and the groove

Make rings in a few standard cord thicknesses and keep to them, so any ring fits any groove (Precision and Interchangeable Parts): 1.78, 2.62, 3.53, 5.33 and 6.99 mm (the old inch sizes, used worldwide).

Static seal (flange, lid, plug) Moving seal (piston, rod)
Squeeze of the cord 20–30 % 10–20 %
Groove depth 0.72–0.80 × cord 0.80–0.88 × cord
Groove width 1.3–1.5 × cord 1.3–1.5 × cord
Example, 3.53 mm cord 2.6–2.8 mm deep, 4.8 mm wide 2.9–3.1 mm deep, 4.8 mm wide
Surface the ring touches Finely turned, marks running round Polished to a mirror

Rules that prevent most failures:

  • Fill no more than 85 % of the groove's cross-section, leaving room to swell.
  • Stretch a ring on a piston or plug 1–5 %: snug, never slack, never more.
  • Gap between moving parts under about 0.1 mm for a 70-hardness ring at 100 bar; beyond that, harder rubber or a backup ring of leather or hard plastic on the low-pressure side.
  • Lead-in: a 15–20° chamfer on bores and shafts, every edge rounded, threads covered with tape on assembly. Grease thinly.

Making an O-ring mould

Lower plate, from above Section through both plates, opened Dowel holes reamed through both Pry slot Half-round cavity turned with a form tool Overflow grooves (dashed) inside and out heated press, 150–180 °C Preform 5–10 % extra Dowel Plates 12–20 mm thick, cavities enlarged 1.5–4 % for shrinkage Closed, one cavity enlarged land 1–1.5 mm Overflow groove 1 mm wide, 0.5 mm deep Flash thin skin: tear off, trim
Fig. 3 A two-plate O-ring mould, exploded. The lower and upper steel plates each have a half-round groove turned in the face, matching exactly. Narrow overflow grooves inside and outside the cavity take the extra rubber. Two dowel pins keep the halves aligned. A cord of uncured rubber is laid in the lower groove; when pressed and cured it becomes a ring with a thin flash at the parting line, which is trimmed off.
  1. Plates. Two plates of mild steel or aluminium, 12–20 mm thick, faces turned flat and true (The Lathe). Drill and ream them together for two or three dowel pins, and cut pry slots in the edges for opening.
  2. Cavity. On the lathe faceplate, turn a half-round groove in each face with a form tool ground to the cord radius (Sharpening and Honing). The two must match in diameter within 0.05 mm, or the ring has a step.
  3. Shrinkage. Make the cavity larger than the finished ring, in both diameter and cord, by 1.5–2 % for nitrile and natural rubber, 3–4 % for post-cured silicone.
  4. Overflow. Leave a flat land 1–1.5 mm wide beside the cavity, then an overflow groove about 1 mm wide and 0.5 mm deep each side. Excess spills into it through flash so thin it tears off.
  5. Polish the cavity to a mirror (Abrasives and Grinding Stones); every scratch prints on the ring. One pair of plates can carry several cavities.

Moulding and curing

  1. Cut a preform of compound cord 5–10 % larger in volume than the cavity. Too little leaves unfilled patches; too much, thick flash.
  2. Lay it in the lower groove of the preheated mould and close the plates in the heated press.
  3. Bump: release and reapply pressure once or twice in the first half-minute to let air out.
  4. Cure with the plates held fully closed: nitrile 8–15 minutes at 160 °C for a 3.5 mm cord; silicone 5–10 minutes at 170 °C, then post-cure; natural rubber as in Rubber. Add about 2 minutes per extra millimetre of cord.
  5. Peel out the ring while hot. Deflash by pulling off the flash and trimming the parting line with sharp curved scissors, never leaving a nick.

Big rings for tank lids and doors are made from cord: cut it square, join the ends with a little uncured compound in a small heated splicing block grooved like the mould, and cure the joint for the same time. A spliced ring is good for static seals only.

Good and bad O-rings

  • Look under a lens: round and glossy, with no bubbles, unfilled dents, flash over 0.1 mm or step at the parting line. Measure the cord at four places: within ±0.08 mm. Stretch it to twice its diameter: it comes back fully, with no white streaks.
  • Compression set, the life test: clamp sample rings between plates with spacers at three-quarters of the cord thickness, at 100 °C for a day (oven or boiling water). Unclamp and measure after half an hour. A good ring recovers at least three-quarters of the squeeze; one that stays flat will leak.
  • Swell test: soak a weighed ring three days in the oil or fuel it will meet. Under 10–15 % gain is good; soft and swollen means the wrong rubber.
  • Which rubber? Burn a sliver. Natural and nitrile burn on, sooty; neoprene puts itself out and smells of hydrochloric acid; silicone burns bright white and leaves white ash. Store rings sealed, dark, and away from motors, whose sparks make ozone.

Note Troubleshooting O-rings. Leaks with no damage → too little squeeze (groove too deep) or a scratch across the sealing face. Check depth; polish the face. Ring flattened square, leaks when cold → compression set: wrong rubber, too hot, or undercured. Post-cure silicone; cure nitrile longer. Edge nibbled to a fringe on the low-pressure side → extrusion into the gap. Reduce clearance, use harder rubber or a backup ring. Ring swollen, soft, rolled out of the groove → wrong rubber for the fluid. See the table. Spiral twist marks on a piston ring → too long a stroke without lubrication, or an uneven groove. Grease it; check the groove. Moulded rings with dull, unfilled patches → preform too small, air trapped (bump more), or mould too cool.

Dangers

Danger Methyl chloride is a flammable, almost odourless gas that damages brain and nerves without warning. Chlorosilanes react violently with water, throwing out choking hydrogen chloride (Hydrochloric Acid); fine silicon dust can explode. Butadiene, chloroprene and acrylonitrile are flammable, poison through skin and lungs, and cause cancer. All belong only in sealed, ventilated works. Peroxides for curing can decompose violently if warmed or contaminated. Keep them cool and weigh out only what you need.

  • Hot presses crush and burn: guards and two-hand controls (Presses, Punches and Dies). Vent post-cure ovens outdoors. Wear a mask when mixing fumed silica.
  • Burning neoprene gives hydrogen chloride, fluoroelastomer hydrogen fluoride: never burn scrap seals indoors.
  • A seal failure can kill. Use the right rubber for every fluid, and replace rings in brakes, gas lines and breathing equipment at the first hardening, cracking or set (Diving and Underwater Work).

What this unlocks

How it was first done

Charles Friedel and James Crafts made the first compound of silicon and carbon in Paris in 1863. Frederic Kipping at Nottingham studied them for forty years from 1899 and named them "silicones", thinking wrongly that they resembled ketones. James Franklin Hyde at Corning made the first useful silicone resins in the 1930s; Eugene Rochow at General Electric found the direct process in 1940, and Richard Müller in Germany independently soon after. Dow Corning was founded in 1943 to supply grease for aircraft ignition systems.

In 1930 Arnold Collins, in Wallace Carothers' group at DuPont, working from Julius Nieuwland's acetylene chemistry, found that chloroprene set to a rubber, sold from 1931 as DuPrene, later neoprene. Erich Konrad and Eduard Tschunkur at IG Farben patented nitrile rubber in 1934. Niels Christensen patented the O-ring in the United States in the late 1930s. In 1986 the space shuttle Challenger broke apart after cold stiffened the O-rings in a booster joint — test every seal at the coldest temperature it will meet.