◆ Rebuild

Part 6 · Building

Reinforced Concrete

Concrete is as strong as stone when squeezed but cracks easily when stretched. Cast steel bars inside it, in the right places, and you get a material that can span a room, hold up a floor, roof a cistern or carry a bridge. How to place the bars, build the formwork, mix, pour, cure and test it.

Difficulty
●●●●●
Time
A lintel in a day plus a week's curing; a floor slab takes a team a week to form and pour, and a month before it carries full load
Steps from zero
23 prerequisites →

You need first

Portland CementSteel in Quantity

This unlocks

Steel Frames and Tall Buildings
The full path from nothing — 23 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. The Kiln
  9. Charcoal
  10. Hides and Leather
  11. Lime
  12. Bricks
  13. The Wheel and Axle
  14. Portland Cement
  15. Firebrick and Refractories
  16. Bellows
  17. Gears
  18. Iron (the Bloomery)
  19. The Waterwheel
  20. The Blast Furnace and Cast Iron
  21. Blacksmithing
  22. Steel
  23. Steel in Quantity
  24. Reinforced Concrete

Do them roughly in this order. See it on the tech tree →

Why it matters

Stone, brick and plain concrete are strong when squeezed and weak when stretched. That is why masonry spans openings with arches (Arches, Vaults and Domes) and why a stone lintel longer than about 2 m tends to crack. Steel is the opposite kind of material: a thin bar can hold several tonnes in pull, but a long thin bar bends easily when pushed.

Put the two together and each covers the other's weakness. Reinforced concrete (concrete with steel bars cast inside) can be poured into almost any shape: flat floor slabs, beams, columns, foundations, water tanks, pipes, retaining walls, bridges and dams. It does not burn, rot or rust (if made well), and it needs no skilled carving — only care, formwork and the right bars in the right places. Most of the buildings and much of the infrastructure of the modern world are made of it.

How it works

Where a beam is stretched

Lay a plank across two bricks and stand on its middle. It sags. The top of the plank is squeezed shorter (compression) and the bottom is stretched longer (tension). Concrete is about ten times stronger in compression than in tension, so a plain concrete beam cracks at the bottom under a load it could easily carry on top. Put steel bars near the bottom and they take the stretching. The concrete still cracks a little — in fine hairlines you can barely see — but the steel holds the cracks closed and the beam carries its load.

So the whole art is putting the steel where the concrete is stretched:

  • A beam or slab resting on two supports: stretched along the bottom.
  • A cantilever (a beam or balcony fixed at one end only): stretched along the top.
  • A beam or slab running continuously over a support: stretched along the top over the support and the bottom in between.
  • Near the supports, the beam also tends to crack in a diagonal line (shear). Steel loops called stirrups (or links) wrapped round the main bars hold it together. They are placed closest together near the supports.
  • A column is mainly squeezed; its bars help carry load and stop it bursting or bending, and ties round them stop the bars buckling outward.
Plain concrete beam top is squeezed (concrete is strong); bottom is stretched and cracks squeezed stretched Beam on two supports main bars at the bottom, hooked up at the ends; stirrups closer together near the supports cover 25–40 mm Cantilever the top is stretched, so the main bars go at the top and run deep into the support stretched
Fig. 1 Where the steel goes. A plain beam cracks along its stretched bottom. In a beam on two supports the main bars run along the bottom, with stirrups closest together near the supports. In a cantilever, the top is stretched, so the main bars go at the top and anchor deep into the support.

Why steel and concrete get along

Three lucky facts make the partnership work:

  1. They expand alike with heat. Both grow by about 1 mm per 100 m for each degree; hot days do not tear them apart.
  2. Concrete grips steel. As cement sets it shrinks onto the bars. Ribs, twists or hooked ends on the bars stop them pulling out.
  3. Concrete protects steel. Wet cement is strongly alkaline (see Lye and Potash), and steel buried in alkaline concrete does not rust. Over decades the outer surface of the concrete slowly reacts with carbon dioxide in the air and loses this protection, a front that creeps inward perhaps 1–2 cm in the first few decades in good concrete, faster in porous concrete. That is why the bars need a cover of concrete: if the cover is too thin, the bars rust, swell and burst the concrete off.

Lime concrete (Mortar and Concrete) does not protect steel this way and is too weak to grip it. You need portland cement (Portland Cement).

What you need

Item Amount / size See
Portland cement About 300–350 kg (6–7 bags of 50 kg) per m³ of concrete Portland Cement
Clean sharp sand About 0.45 m³ per m³ of concrete Mortar and Concrete
Gravel or crushed stone Up to 20 mm; about 0.9 m³ per m³
Clean water About half the weight of the cement
Steel bars 6–8 mm (stirrups, ties, slab cross-bars); 10–20 mm (main bars) Steel in Quantity
Soft iron tying wire 1–1.5 mm, annealed Copper Wire (same drawing method)
Planks, timber, nails, wedges Formwork and props Timber Framing and Log Building, Nails, Rivets and Wire Fasteners
Spacer blocks Small cubes of mortar, 25–50 mm thick, with a wire cast in
Mixing board, shovels, buckets, rammers

Bar weight: a steel bar weighs about (diameter in mm)² ÷ 162 kg per metre. A 12 mm bar weighs 0.89 kg/m; a 16 mm bar 1.58 kg/m.

Where to find it

  • Cement: limestone or chalk burned with clay, as in Portland Cement.
  • Steel bars: rolled from mild steel billets in a rolling mill (Sheet Metal and Rolling), or forged by hand from mild steel or wrought iron — slow, but a smith can draw out a few metres of 10–12 mm rod a day. Mild steel (soft, low-carbon) is right: it bends without cracking and stretches before it breaks, giving warning. Do not use hard, high-carbon steel that snaps when bent. Bars salvaged from ruins are excellent if they are not deeply rusted — but the from-scratch route is Steel in Quantity.
  • Making bars grip: modern bars are rolled with ribs. Without ribs, give plain round bars a hook at each end (a full half-turn bent round a pin four times the bar thickness), or twist square bars cold, a turn every 15–20 cm, as the American builder Ernest Ransome did in the 1880s.
  • Aggregate: river gravel or crushed hard stone, washed free of clay and silt. Sand must be sharp and clean (Mortar and Concrete). Never use sea sand or salty water: salt rusts the steel.

Step by step

1. Decide the sizes

Large structures need real calculation (see Strength of Materials) and a load test. In earthquake country, columns and beam ends need extra ties and laps (Building Against Earthquakes and Storms). For small buildings, these rules of thumb are a starting point, for floors in houses (a load of about 200 kg per m² for people and furniture, on top of the floor's own weight) and mild steel bars:

Member Size Steel
Lintel over a door or window, up to 2 m Depth at least 1/10 of the span, never less than 15 cm; as wide as the wall 2 bars of 12 mm at the bottom, 2 of 8–10 mm at the top; 6 mm stirrups every 15 cm
Floor slab on two supports, up to 4 m span Thickness 1/25 of the span, at least 10 cm (14 cm for 3.5 m) 10 mm bars every 10 cm along the span, at the bottom; 8 mm bars every 25 cm across them
Beam on two supports, up to 5 m span Depth 1/12 of the span, width about half the depth (4 m span: 35 cm deep, 20 cm wide) Bottom bars about 1–1.5% of width × depth (4 bars of 18 mm for the 4 m beam); 2 bars of 12 mm on top; 8 mm stirrups every 12 cm near the ends, 20 cm in the middle
Column, one or two storeys At least 25 × 25 cm 4 bars of 12–16 mm, one in each corner; 6 mm ties every 15 cm
Cantilever (balcony) Depth at least 1/7 of its reach Main bars at the top, running into the support at least as far as the cantilever reaches

Cover (concrete between the bars and the outside surface):

Where Cover
Indoor slabs 20–25 mm
Indoor beams and columns 25–40 mm
Outdoors, or in water tanks 40–50 mm
Against the earth (footings) 75 mm

2. Cut, bend and tie the steel

  1. Cut bars with a hot chisel on an anvil, or a cold chisel and a heavy hammer.
  2. Bend cold round a pin set in a heavy bench — a pin 2–3 bar diameters thick for stirrups, 4 diameters for main bars — using a bar of pipe slipped over the end as a lever. Never bend a bar back and forth, and never heat mild steel bars to bend them in the field: you change their strength unpredictably.
  3. Laps: where one bar ends and another continues, overlap them by 50 bar diameters (60 cm for 12 mm bars), tied together, with hooks on plain bars. Stagger laps so they do not all fall in one place, and keep them away from the middle of beams.
  4. Tie every crossing with a short loop of soft iron wire, twisted tight with pliers or a hooked stick. The cage of bars must be stiff enough that people can walk on it without displacing it.
  5. Set spacers — mortar blocks of the cover thickness, every 1 m or so — under the bottom bars and against the sides, tied on with their wires. Without them the bars sink to the bottom of the form and have no cover.

3. Build the formwork

Formwork (also called shuttering) is the temporary mould. It must hold the shape, the weight and the pressure of the wet concrete, which weighs 2.4 tonnes per m³: a 15 cm slab weighs 360 kg per m², before the workers on it.

Slab and beam formwork, in section Deck boardsoiled, tight joints slab bars Stirrup Main beam barson spacer blocks slab 10–15 cm joists bearers Beam boxkickers holdthe sides side board Props1 m apart,braced wedges on sole plates:knock out to strike
Fig. 2 Formwork for a floor slab and beam, seen in section. Deck boards sit on joists, which sit on bearers carried by props on wedges and sole plates. The beam is cast in a box of boards. The bars sit on spacer blocks so they are surrounded by concrete.
  1. Deck boards 25–30 mm thick, planed on the face side and laid with tight joints, on joists (about 5 × 10 cm) at 50 cm centres, on bearers (about 10 × 15 cm) at 1–1.2 m, on props (10 × 10 cm squared timber or round poles 10–12 cm thick) at about 1 m centres.
  2. Props stand on wedges on sole plates — short planks spreading the load on the ground. The wedges let you adjust the height and later knock them out to lower the form gently. Brace the props diagonally both ways.
  3. Beam boxes of boards with a bottom board and two sides, held at the foot by kickers (cleats) nailed to the supports and at the top by the slab deck.
  4. Camber: set the middle of each span a little high — about 2 mm per metre of span — so the finished floor is level after it settles.
  5. Seal and oil. Fill gaps with clay, paper or strips of tin so the cement paste cannot run out (leaks leave stony, honeycombed patches). Brush the inside with old oil, soft soap or limewash so concrete does not stick. Wet the timber before pouring.
  6. Check everything with level and plumb line (Surveying and Levelling), then check the props again.

4. Mix and pour

  1. Mix: 1 cement : 2 sand : 4 gravel by volume for slabs and footings; 1 : 1½ : 3 for beams, columns and water tanks. Mix dry on a board until the colour is even, make a hollow, add water a little at a time and turn until every stone is coated and the mix is like stiff porridge. Use the least water that lets you work it into the forms — a sloppy mix can be half as strong. Place it within an hour.
  2. Slump test: fill a sheet-metal cone 30 cm high (10 cm across the top, 20 cm across the bottom) in three layers, rodding each 25 times; lift the cone straight up and measure how far the heap sinks. 2.5–7.5 cm is right for slabs and beams. More means too much water.
  3. Pour without stopping if you can. Start at the far end and work back. Do not drop concrete more than about 1.5 m or the stones separate from the paste; for tall columns, fill through a hole in the side of the form, or down a chute.
  4. Compact every layer (no more than 30 cm deep in beams and columns) by pushing a rod or thin bar up and down through it, and by tapping the formwork with a mallet until air bubbles stop rising and a film of paste shows at the surface. Work it well round the bars and into the corners.
  5. Stop at the right place. If a pour must stop, end it with a vertical board across the middle third of a slab or beam span, never near a support. Before continuing, roughen the old face, wash it, and brush on a thin cement slurry.
  6. Finish the top of slabs with a straight board pulled back and forth across the forms, then a wooden float.

5. Cure and strike

  1. Keep it wet for at least 7 days, better 14. Cover with wet sacks, straw or sand, and sprinkle three times a day; shade it from sun and wind. Concrete that dries early never reaches its strength.
  2. Strike (remove) the formwork gently by knocking out the wedges, never by prising. At ordinary temperatures (15–20 °C):
Formwork Earliest removal
Sides of beams, columns and walls 2 days
Slab deck boards (put props straight back under) 7 days
Props under slabs 14 days
Props under beams 21 days

Double these times below 10 °C. No concreting at all if frost is expected within a few days.

  1. Do not load a slab or beam with its full load for 28 days. Concrete reaches about two-thirds of its final strength in a week and most of it in a month.

The easiest first project: ferrocement

Ferrocement — a thin shell of rich cement mortar packed into several layers of fine wire mesh — needs no big formwork and no heavy bars. It is excellent for water tanks (Wells and Cisterns), troughs, roof shells and even boats.

  1. Build a skeleton of 6 mm bars about 10–15 cm apart in the shape you want (for a tank: a cylinder of vertical bars and horizontal rings).
  2. Tie two to four layers of fine wire mesh (woven or hexagonal netting of 1 mm wire, openings 1–2 cm) tightly to both faces.
  3. Press in a stiff mortar of 1 cement : 2 sand, with very little water, from both sides at once if you can, until the mesh is completely filled and covered by about 5 mm. The finished wall is 2.5–4 cm thick.
  4. Cure it wet for two weeks. A 10,000-litre ferrocement tank uses only a few bags of cement.

How to tell it worked

  • Clean faces after striking: smooth, with no honeycombed patches of loose stones, no bars showing. Small honeycombs can be cut back and filled with rich mortar; large ones mean the member is weak and must be judged by a load test.
  • Ring test: tap with a hammer. Good concrete rings; hollow or poorly compacted areas sound dull.
  • Load test (for any important slab or beam, after 28 days): stretch a string tight under the middle of the span, fixed at the supports, and measure from it to the underside. Load the floor evenly with sandbags, bricks or water in lined pits to 1¼ times the load it is meant to carry for 24 hours. The middle should sag less than 1/250 of the span (16 mm for 4 m), with no cracks wider than a hair, and at least three-quarters of the sag should recover within a day after the load is removed.
  • Test bars before use: a sample of each batch of bars should bend cold round a pin of twice its thickness to 180° without cracking.

Note Troubleshooting. Honeycombed patches → mix too dry or too stony, not compacted, or paste leaked from the forms. Seal joints, tap the forms, rod each layer. Fine cracks all over the surface within a day → dried too fast. Shade and wet it sooner and longer. Wide crack across the middle of a beam's underside → too little bottom steel, or bars too high in the beam. Prop it and do not load it; it must be strengthened or rebuilt. Diagonal cracks near the supports → not enough stirrups. Prop it at once. Rust stains and flakes of concrete falling off (years later) → too little cover or a porous mix. Cut back to clean steel, paint the bars with cement slurry and patch with rich mortar. Formwork bulged during the pour → too few props or ties. Stop pouring, prop it, and reduce the rate of filling.

Dangers

Danger Formwork collapse during the pour is the commonest way people die building in concrete. Wet concrete is very heavy and the load grows quickly while workers stand on top. Props that are too thin, too far apart, unbraced, or standing on soft ground can fold suddenly and drop everything, and everyone, into the space below. Over-design the props, brace them both ways, stand them on sole plates, inspect them during the pour, and keep everyone not needed out from underneath.

Danger Striking too early. A slab or beam that looks hard after a few days may still be far too weak to stand alone. Removing props early has dropped whole floors. Follow the striking times, double them in cold weather, and never stand under a span while the last props are removed — knock them out from the side with a long pole.

  • Cement burns: wet cement is as caustic as Lye and Potash. It burns skin, especially knees and inside boots, and can blind. Wear gloves and eye protection, cover arms and legs, and flush splashes with plenty of water at once (Portland Cement).
  • Bar ends: upward-pointing bars impale people who fall onto them. Bend the ends over or cap them with a block of wood.
  • Heavy lifting: a bag of cement weighs 50 kg, a bucket of concrete 25–30 kg. Lift with your legs and share loads; use hoists (Cranes and Lifting) for anything going up.

What this unlocks

Reinforced concrete makes fireproof floors and roofs, strong Foundations and Floors, water tanks and cisterns (Wells and Cisterns), Sewers and Wastewater and culverts, bridges (Roads and Bridges), dams (Dams and Reservoirs) for hydroelectric power, harbour walls, and the floors and cores of Steel Frames and Tall Buildings. Pre-casting — making beams, pipes, posts and slabs on the ground and lifting them into place with Cranes and Lifting — speeds building enormously.

How it was first done

In about 1848 Joseph-Louis Lambot in southern France built small boats from cement mortar spread over iron mesh — the first ferrocement — and showed one at the Paris Exhibition of 1855. In 1854 William Wilkinson of Newcastle, England, patented floors with iron bars or old wire ropes cast in the stretched part of the concrete. The Paris gardener Joseph Monier patented reinforced plant tubs in 1867 and later pipes, tanks and bridges. In 1877 the American Thaddeus Hyatt published tests showing that the iron belongs on the tension side. François Hennebique of France patented a complete system of columns, beams with stirrups, and slabs in 1892 and licensed it across the world; and in 1903 the 16-storey Ingalls Building in Cincinnati, USA, became the first reinforced concrete skyscraper. Since then, reinforced concrete has become the most used building material on Earth.

Source: content/entries/building/reinforced-concrete.md