◆ Rebuild

Part 2 · Earth and Fire

Glass

How to melt sand with plant-ash alkali and lime into glass, in a clay crucible at 1,100–1,200 °C, and how to cast it, blow it and anneal it so it does not crack. Glass gives you windows, bottles, lenses and the vessels of chemistry.

Difficulty
●●●●●
Time
Weeks to build and dry furnace and crucibles; a day or two per melt; many attempts
Steps from zero
6 prerequisites →

You need first

The KilnLimeLye and Potash

This unlocks

Window GlassLaboratory GlasswareSulfuric AcidGlass Fibre and Glass WoolBottles, Drinking Glasses and GlasswareGlazesScientific Glassblowing and Glass-to-Metal SealsThe Light BulbStatic Electricity and the Leyden JarSolar HeatCanning and BottlingPenicillinHourglasses, Water Clocks and Simple TimersLensesMirrorsOptical Glass and Achromatic LensesThe Spectroscope
The full path from nothing — 6 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. The Kiln
  4. Pottery
  5. Lime
  6. Lye and Potash
  7. Glass

Do them roughly in this order. See it on the tech tree →

Why it matters

Glass is melted sand that has forgotten to crystallise. It is clear, waterproof, and resists almost every chemical. It can be shaped while hot into almost anything, and ground when cold into lenses.

With glass you can make:

Glass is also one of the hardest things in this part of the book. It needs the highest temperatures, good crucibles, carefully prepared ingredients, and patience. Expect your first melts to be bubbly, green and cracked. That is how glass looked for its first two thousand years, and it was still enormously useful.

How it works

The main ingredient of glass is silica — quartz, the mineral that makes up most sand. Pure silica melts only at about 1,700 °C, far beyond any wood fire. Two other ingredients make glass possible:

SANDabout 70% the former:builds the glass FLUX15–20% soda or potash:sand melts at ~1,100 °Cinstead of 1,700 °C LIMEabout 10% the stabiliser:hard, will notdissolve GLASS 1,100–1,250 °Cyellow heat, for hours proportions of the finished glass, by weight
Fig. 1 The three ingredients of glass. Sand forms the glass; alkali flux lets it melt at kiln temperatures; lime makes it hard and stops it dissolving in water.
  1. The former — silica (sand or crushed quartz). About 70% of the finished glass. It makes the glassy network.
  2. The flux — an alkali. About 15–20%. A flux is a substance that helps another melt at a lower temperature. Soda (sodium carbonate) or potash (potassium carbonate), both made from plant ashes (see Lye and Potash and Soda Ash and Baking Soda), bring the melting point of sand down to about 1,100 °C.
  3. The stabiliser — lime. About 10%. Glass made of only sand and alkali dissolves slowly in water (it is called "water glass"). Lime (calcium oxide, from limestone or shells — see Lime) makes the glass hard, durable and insoluble.

Glass has no exact melting point. It softens gradually:

Temperature Colour of glow State of the glass
1,100–1,250 °C Yellow-orange to yellow Batch melts and bubbles clear; runny like honey
950–1,100 °C Orange Working range: thick like cold honey, can be gathered and blown
700–900 °C Cherry red Stiff; can be bent but not blown
About 520–550 °C Just at the edge of visible glow in the dark Annealing: hard, but stresses can relax
Below 500 °C No glow Rigid; can crack if cooled unevenly

A piece of glass cools from the outside in. If it cools quickly, the outside sets hard while the inside is still shrinking, and the glass is left full of locked-in stress. It may crack on the spot, or days later, for no visible reason. Annealing — holding the glass at about 520 °C and then cooling it very slowly — lets those stresses relax. Every piece of glass must be annealed.

What you need

Item Amount Notes
Clean, white sand or crushed quartz 1–2 kg per melt See "Where to find it"
Alkali flux 0.4–0.8 kg per melt Soda ash, purified potash (see Lye and Potash), or plant ash
Lime 0.2–0.5 kg per melt Crushed limestone, burnt shells, or quicklime (see Lime)
Fireclay and grog Several kg For crucibles (below)
A furnace that holds 1,100–1,250 °C for hours 1 Charcoal and bellows (below), or a large wood-fired glass furnace
Charcoal 20–50 kg per firing For the charcoal furnace
Bellows 1–2 For the charcoal furnace
An annealing oven 1 A small kiln, or a pot of hot ash (below)
Iron tools For blowing Blowpipe, solid rod (punty), tongs, shears — see Blacksmithing
Flat smooth stone 1 The marver, for rolling hot glass
Wooden paddles and blocks Several Kept soaking in water
A stone or clay mortar 1 For grinding batch

Where to find it

  • Sand. You want sand that is nearly pure quartz: white or very pale, with clear, glassy grains under a lens or in bright sun. Look on beaches and in dunes below white cliffs, in riverbeds draining sandstone or granite country, and in pale sandstone (crush it). Yellow, red and brown sand contains iron, which colours glass green or brown — usable, but not clear. Dark grains (often magnetic iron minerals) are worse.
  • Quartz pebbles and veins. Milky-white quartz occurs as pebbles in rivers and as veins in other rocks. It is very pure silica. Heat pebbles to red heat in a fire and drop them into cold water: they crackle into pieces that are easy to crush. Venetian glassmakers made their finest glass from crushed white river pebbles.
  • Alkali. Wood ash and fern ash give potash; leached and purified, they give fairly pure potash (see Lye and Potash). Ash from salt-marsh plants — glasswort, saltwort and kelp (seaweed) — gives soda, which makes better glass. Dry lake crusts that taste soapy are natural soda (natron). See Soda Ash and Baking Soda.
  • Lime. Limestone, chalk or seashells, crushed; or quicklime from your Lime kiln.

Preparing sand. Wash it in a basket in running water until the water runs clear, removing clay and dust. Pick or float out dark grains and plant matter. Dry it. Grind it finer in a mortar if the grains are coarser than about 0.5 mm, and sieve. Fine sand melts much faster.

The batch: recipes

All recipes are by weight. Weigh on a simple balance (see Measurement from Scratch). Mix very thoroughly — grind everything together in a mortar for best results.

Recipe Sand Flux Lime Result
Soda-lime (the best start) 100 35 soda ash 25 crushed limestone or shell (or 14 quicklime) Clear to pale green, durable, easiest to work
Potash-lime 100 40 purified potash 25 crushed limestone or shell (or 14 quicklime) Harder, stiffer; melts a little hotter
Forest glass (from raw ash) 1 part 2 parts sifted hardwood ash, by volume none — the ash contains lime Green to brown; how medieval Europe made its glass
Plant-ash soda 2 parts 1 part ash of glasswort or saltwort, by weight usually none Pale green; ancient Near Eastern glass. Test and adjust

Notes:

  • The forest glass recipe comes from a 12th-century monk, Theophilus, who wrote: two parts beech-wood ash to one part sand. Wood ash varies a lot; if the batch will not melt, add more ash; if the glass later turns cloudy in water, add more sand.
  • Limestone and shells give off gas as they heat, so the batch foams. Quicklime avoids this but is caustic to handle (see Lime).
  • Add broken glass (called cullet) from earlier melts: up to a third of the batch. It melts first and helps everything else melt faster.
  • Fritting (optional but helpful): heat the mixed batch in a shallow clay dish at bright red heat (800–900 °C) for several hours, stirring, until it becomes a sintered, spongy cake. Crush it and use it as your batch. Much of the gas and foam is gone, and it melts faster and cleaner.

Crucibles

A crucible is a pot that holds the molten glass. It must survive 1,200 °C for many hours without softening, cracking or being eaten away by the alkali.

  1. Clay. Use the most heat-resistant clay you can find: white or pale grey clays that stay pale when fired (fireclay or kaolin — see Finding and Preparing Clay and Firebrick and Refractories). Red-firing clays soften at these temperatures.
  2. Mix 1 part clay with 1 part grog (crushed fired crucible or pale pottery), by volume. Wedge it very well.
  3. Shape a thick pinch or coil pot: walls and base 1.5–2 cm thick, about 10–15 cm across and 12–15 cm tall for a first crucible (holding about 1 kg of glass). Round the inside bottom; no sharp corners.
  4. Dry it slowly for at least two weeks, then fire it in your The Kiln to the highest heat you can reach.
  5. Always preheat a crucible before putting it into a hot furnace — set it near the furnace mouth for an hour, then move it in gradually.

Make several. Crucibles crack and wear out; a typical early crucible lasts a few melts.

Building the furnace

Wood fires struggle to hold 1,150 °C. Two ways to get there:

Option A: Charcoal furnace with bellows (best for a first glass)

Glory holein the lid: gather glassand reheat pieces here Charcoalwalnut-sized,kept topped up Bellowstwo, in turn Air pipeclay, 3–4 cm bore Cruciblefireclay + grog,walls 1.5–2 cm Meltyellow heat,1,100–1,250 °C Standcrucible clear of the blast CHARCOAL FURNACE ANNEALING OVEN pieces go in while hot;held at 500–550 °C,a dull glow seen in shade;then sealed for 12–24 h embers keep it warm
Fig. 2 A small charcoal glass furnace in cross-section, with a separate annealing oven. Bellows blow air through a clay pipe into a bed of charcoal around the crucible. Finished pieces go straight into the annealing oven, which is held at a dull red heat and then sealed to cool slowly.
  1. Build a round furnace of the heat-resistant kiln mix from The Kiln — but with more grog, and fireclay if you have it — with an inside diameter of about 30 cm, walls 10–15 cm thick, and about 40–50 cm tall. Bank earth around the outside.
  2. About 10 cm above the floor, set a clay air pipe (a tuyère, 3–4 cm bore) through the wall, angled slightly down, and connect it to one or two Bellows working in turn so the air never stops.
  3. Make a lid of clay with a hole 8–10 cm across. This hole is your working hole (glory hole): you gather glass through it and reheat pieces in it.
  4. Set the crucible on a clay or brick block so that its base is just above the air pipe — not directly in front of the blast, which would crack it.
  5. Fill around it with charcoal broken to walnut size.

With steady bellows work, a charcoal furnace like this reaches 1,200–1,300 °C — bright yellow. It needs a team to pump the bellows in shifts and to keep adding charcoal.

Option B: A wood-fired glass furnace

Historic glasshouses used a large beehive-shaped fireclay furnace: a firebox below, several crucibles on a bench inside, a working hole in front of each, and an annealing chamber heated by the waste heat. It burned very dry, thinly split wood day and night for weeks. It makes glass in quantity, but needs a skilled team and a forest of wood. Start with Option A.

The annealing oven

Build a small chamber — a box or a dome of kiln mix with a door, about 30–40 cm inside — that you can heat with a few embers or a small fire to a dull red glow, visible only in shade: about 500–550 °C. A small pottery The Kiln serves. In a pinch, use a large clay pot filled with hot wood ash and embers, kept beside the furnace.

Step by step: making glass

  1. Preheat everything. Light the furnace gently, with the crucible already inside (or preheat it separately). Bring it up slowly over 2–3 hours to orange heat. A crucible heated fast will crack.
  2. Go hot. Work the bellows steadily until the inside of the furnace glows yellow-orange to yellow (1,100–1,200 °C or more). Light the annealing oven.
  3. Charge the batch in portions. Using a long-handled clay or iron ladle, add about a third of the batch. It will sinter, foam and slowly sink into a sticky, bubbling melt. Wait until it has melted down — 30–60 minutes — before adding the next third. Add the rest the same way. Fill the crucible no more than two-thirds full, because the batch foams up.
  4. Melt and fine. Keep the furnace at full heat for 4–8 hours more. Bubbles slowly rise and burst ("fining"). A white, frothy scum may float on top ("glass gall") — skim it off with an iron ladle or a clay spoon.
  5. Test. Dip a preheated iron rod into the melt and pull out a thread. Let it cool. It should be glassy and clear (it may be green or brown, and have a few bubbles). White grains in it are unmelted sand — keep melting, hotter and longer. If it never clears, the batch needs more flux.
  6. Choose how to shape it (below). Let the furnace drop slightly, to orange heat, so the glass is thick enough to work.
  7. Anneal every piece (below).
  8. Shut down. When finished, you can leave the remaining glass in the crucible and let the furnace cool slowly; break the crucible later and keep the glass as cullet.

Shaping glass

Casting (the simplest)

  • Slabs. Ladle or pour molten glass onto a preheated flat stone dusted with fine ash, or into a shallow tray of fine dry sand. Press flat with a wet wooden paddle. Move it to the annealer at once.
  • Moulds. Pour into a preheated mould of clay or stone (a bowl shape, a lens blank, a block). Or put lumps of cullet into a clay mould and heat them in a kiln until they slump and fuse.
  • Lens blanks cast this way can later be ground and polished (see Lenses).

Beads and rods

Gather a little glass on an iron rod, pull it into a thread, and wind the soft thread around a thin metal rod coated with a paste of clay and water (so the bead slides off when cold). Glass rods and threads pulled from the melt cool into canes you can remelt later in a flame.

Blowing

Blowing needs an iron blowpipe: a tube about 1.2–1.5 m long with a bore of about 1 cm, often with a wooden grip in the middle. It needs a skilled smith (see Blacksmithing), and the glassblower needs months of practice.

turn roll on the stone puff thumb wet wooden paddle drop of watercracks it off punty 1 GATHERhot pipe end,turn to wind it on 2 MARVERround and even;keep turning 3 BLOWpuff, cap with thumb;hot air opens a bubble 4 SHAPEreheat, blow andshape with wet wood 5 PUNTYrod on the base,crack off the pipe
Fig. 3 Blowing glass. Gather glass on the hot end of the pipe; roll it on the marver; blow a small puff and cap the pipe with your thumb so the trapped air expands; reheat and blow to size, shaping with wet wooden tools; then move the piece onto a punty to finish the open end.
  1. Heat the pipe end in the glory hole to a dull red — cold iron does not grip glass.
  2. Gather. Dip the hot end into the melt and turn the pipe so the glass winds onto it like honey on a spoon. Lift out a lump the size of a walnut. Keep turning the pipe at all times while the glass is soft, or it droops.
  3. Marver. Roll the gather on the flat stone to make it round and even and to stiffen its skin.
  4. First bubble. Blow a short puff into the pipe and cover the mouthpiece with your thumb. The air inside heats, expands and opens a small bubble. Then blow gently while turning.
  5. Reheat and gather more. Return to the glory hole whenever the glass stiffens (when its glow fades to dull red). For larger pieces, dip the first bubble back into the melt to gather more glass over it.
  6. Shape. Blow to size while turning. Shape it with a wet wooden paddle or a cupped wooden block soaked in water — a cushion of steam keeps wood from sticking and burning — and pinch a neck with tongs.
  7. Transfer to the punty. Touch a hot solid iron rod (the punty), with a little blob of glass on its tip, to the bottom of the piece. Touch a wet tool to the neck where it joins the blowpipe, and tap the pipe: the piece cracks off.
  8. Finish. Reheat the open end, widen it with tongs or a wooden stick, and fire-polish the rim in the glory hole.
  9. Anneal. Tap the punty sharply to break the piece off into the annealing oven.

Annealing

  1. Put each piece into the annealing oven while it is still hot — never let it cool in the open air first.
  2. Keep the oven at about 500–550 °C — a dull glow you can just see in shade — for at least 30–60 minutes after the last piece goes in (longer for thick pieces: about an hour per centimetre of thickness).
  3. Seal the oven — close the door and openings with clay — and let the whole thing cool as slowly as possible, at least 12–24 hours. Do not open it until it is cool enough to touch.

How to tell it worked

  • It is glass. Hard, smooth, glassy, transparent or translucent. Bubbles and a green tint are normal for early glass.
  • It survives. A well-annealed piece survives being handled, washed and set down for weeks. Badly annealed glass cracks on its own, sometimes days later, or shatters when lightly scratched.
  • It is stable. Grind a small piece to powder and boil it in clean water for half an hour. The water should not feel slippery or soapy between your fingers. Or leave a piece in water for a week: its surface should stay bright, not turn cloudy, greasy or flaky. Unstable glass has too much flux and too little lime or sand — remake it with more of both.
  • It rings. A good vessel rings when tapped with a fingernail.

Colour.

  • Green, blue-green or brown: iron, from the sand and the ash. Almost all early glass is this colour. Purer sand and quartz give clearer glass.
  • Clear: add about 0.5–1% of finely ground manganese ore (pyrolusite, a soft black mineral that stains fingers — see Finding and Identifying Ores) to cancel the green. Too much turns glass purple.
  • Blue or turquoise: a little copper scale or verdigris (1–2%) — see Copper Smelting.
  • Amber: from sulfur and charcoal in the melt.
  • Opaque white: bone ash or tin oxide.

Note Troubleshooting. Batch does not melt, stays a white crust → not hot enough, or too little flux; work the bellows harder, grind the batch finer, add cullet, or add 10% more flux. Glass full of white specks → unmelted sand ("stones"); melt longer and hotter, use finer sand. Full of bubbles → normal for early glass; melt longer and hotter, let it stand quietly before working, or frit the batch first. Cracks hours or days later → poor annealing; anneal longer and cool slower. Turns cloudy or greasy, or weeps in damp air → unstable glass; more lime and sand, less flux. Crucible cracked or leaked → preheat slower; use more grog and a whiter clay; make walls thicker.

Dangers

Danger Hot glass looks exactly like cold glass. Below about 500 °C it does not glow, but it will still burn you to the bone. Assume every piece of glass near the furnace is hot. Never pick up glass, a tool or a crucible without testing it by holding your hand near it first, and put hot pieces only in their set place.

Danger Molten glass and water. Molten glass spilled onto wet ground or into water can explode in a burst of steam, throwing hot fragments. Keep the ground around the furnace dry and covered with sand. A cracking crucible can dump its contents without warning — keep feet and legs out of the way and wear leather.

  • Eyes. The glare of a glass furnace, looked into for years, causes cataracts — "glassblower's cataract". Look into the glory hole briefly and from the side. Flying shards of glass can blind: shield your eyes when cracking off and breaking pieces.
  • Burns. Wear thick wool or leather, never loose plant-fibre clothing near the furnace — it catches fire. Keep a bucket of water nearby for burns (cool them for 20 minutes) — but never near molten glass.
  • Never breathe in through the blowpipe. You would draw hot air into your lungs. Blow out only.
  • Batch dust. Fine sand and quartz dust cause silicosis (see Finding and Preparing Clay); alkali and lime dust burn eyes and lungs (see Lime). Grind batch wet or outdoors, with a damp cloth over your face.
  • Charcoal furnace fumes contain carbon monoxide. Work outdoors or under an open roof.
  • Lead. Old recipes for "crystal" use lead. Lead fumes and dust poison the brain and blood. Do not use lead.
  • Cuts. Broken glass is razor sharp; sweep and bury waste glass, or keep it as cullet in a closed pot.

What this unlocks

Blown glass gives Bottles, Drinking Glasses and Glassware, and specially purified melts give Optical Glass and Achromatic Lenses. Glass leads straight to Lenses — and through them to the The Microscope and The Telescope. It makes the laboratory possible (Laboratory Glassware, Scientific Glassblowing and Glass-to-Metal Seals): Distillation apparatus, flasks for Sulfuric Acid and Nitric Acid, the The Thermometer, and the glassware of Penicillin. It gives Glazes for pottery, and, with a The Vacuum Pump, the The Light Bulb and the The Vacuum Tube.

How it was first done

Glassy glazes on stone and on beads of quartz paste ("faience") were being made in Egypt and Mesopotamia before 3000 BC, and glass itself was probably first made by accident in such work. Solid glass beads appear in Mesopotamia around 2500 BC, and by 1500 BC workshops in Mesopotamia and Egypt made small glass vessels by winding soft glass around a core of clay and dung. Glassblowing was invented about 50 BC on the coast of what is now Syria, Lebanon and Israel, and the Roman Empire spread cheap blown glass everywhere. (The Roman writer Pliny told a story of sailors who discovered glass by cooking on blocks of soda on a beach; it is probably a legend.) In medieval Europe, glassmakers worked in the forests, using wood ash as flux, and made the "forest glass" of church windows. In 1291 Venice moved its glassmakers to the island of Murano, and in the 15th century they learned to make a nearly colourless glass, cristallo, using purified plant ash and crushed white quartz pebbles.

Source: content/entries/earth/glass.md