Part 13 · Electricity
Fuel Cells
A fuel cell runs electrolysis backwards. Hydrogen and oxygen meet on a catalyst through an electrolyte, and instead of burning they give a steady electric current, with pure water as the only exhaust. How William Grove's gas battery of 1839 works, how to build one on a bench, how the porous gas electrode made the idea practical, the alkaline, phosphoric acid and membrane cells in outline, and an honest look at what fuel cells are good for and what they are not.
- Difficulty
- ●●●●●
- Time
- An afternoon for a Grove cell once you have platinum wire; weeks to make porous electrodes and a small alkaline cell that gives useful power
- Steps from zero
- 28 prerequisites →
This unlocks
—The full path from nothing — 28 steps before this one
- Fire
- Cordage and Rope
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Sulfur
- Hunting and Trapping
- Basic Woodworking
- Charcoal
- Pottery
- The Kiln
- Hides and Leather
- Salt
- Lime
- Fermentation
- Lye and Potash
- Glass
- Bellows
- Saltpeter
- Copper Smelting
- Lead
- Sulfuric Acid
- Gold and Silver
- Nitric Acid
- Hydrochloric Acid
- The Battery
- Platinum and the Platinum Metals
- Electrolysis
- Fuel Cells
Do them roughly in this order. See it on the tech tree →
Why it matters
In Electrolysis you push a current through water and it splits into hydrogen and oxygen. A fuel cell does the opposite: feed it hydrogen and oxygen and it gives the current back, making water. It has no moving parts, no flame and no noise, and it turns the chemical energy of hydrogen into electricity about twice as efficiently as burning hydrogen in an engine to turn a The Generator.
That makes it the right tool for a few special jobs: power in a spacecraft, where the water it makes is drunk by the crew (Spaceflight and Spacecraft); a silent submarine (Helicopters, Rockets and Submarines (Overview)); standby power at a remote radio station; a clean electric vehicle that refuels in minutes (Electric Vehicles). It also teaches you something deep about chemistry: a fire and a battery are the same reaction, one done all at once and one done in a controlled way.
Be honest with yourself before you build one. For storing your own electricity, a The Rechargeable Battery gives back about four-fifths of what you put in; splitting water and running it back through a fuel cell gives back only a third to two-fifths. A fuel cell earns its place when hydrogen is plentiful, or when weight, silence or water matter more than cost.
How it works
Two half-reactions, kept apart. Hydrogen and oxygen want to combine. If they meet, they burn or explode. In a fuel cell they never meet. Hydrogen goes to one electrode, oxygen to another, and an electrolyte — a liquid or solid that lets ions (charged atoms) through but not electrons — lies between them.
- At the hydrogen electrode (the anode, negative terminal), a catalyst splits each hydrogen molecule and strips off its electrons.
- The electrons cannot cross the electrolyte, so they go round through the outside wire, doing work on the way: lighting a lamp, turning a motor.
- At the oxygen electrode (the cathode, positive terminal), oxygen takes up those electrons and, with ions arriving through the electrolyte, becomes water.
In an acid electrolyte, hydrogen ions (protons) carry the charge across and water forms at the oxygen side. In an alkaline one (caustic potash), hydroxide ions carry it the other way and water forms at the hydrogen side. The net result is the same:
hydrogen + oxygen → water + electricity + some heat.
The voltage. The reaction's energy sets the voltage. A perfect hydrogen–oxygen cell at room temperature would give 1.23 volts. Real cells give about 1.0 V with no load, falling to 0.6–0.8 V when working. To get more voltage, connect cells in series, as in any The Battery; to get more current, make them bigger.
The amount (Faraday's law). Every electron comes from the hydrogen, so the current tells you exactly how fast you burn it (Electrolysis gives the law). One ampere for one hour uses about 0.45 litres of hydrogen and 0.23 litres of oxygen at room temperature and makes 0.34 g of water. A cell working at 0.7 V uses about 0.64 m³ of hydrogen for each kilowatt-hour and makes about half a litre of water. Hydrogen holds about 3 kWh per cubic metre as heat, so that is roughly 50% efficient.
The hard part: where three things meet. The reaction can only happen where gas, electrolyte and catalyst all touch at once: the gas must reach the catalyst, and the ions must be able to leave it through the liquid. On a flat metal plate dipped in acid, that is only a thin line where the liquid surface meets the plate. That is why Grove's cell, below, gives only tiny currents. Every advance since has been a way of making this three-phase boundary enormous: rough, porous electrodes full of tiny pores, each with a meniscus of liquid inside it, and catalysts spread as the finest possible dust.
The catalyst. Hydrogen and especially oxygen react slowly at ordinary heat. Platinum (Platinum and the Platinum Metals) is by far the best catalyst for both, especially as platinum black. In alkaline cells, nickel works for hydrogen and silver for oxygen, which is why the alkaline cell is the one a rebuilder can most hope to make in quantity. Hot cells (above 600 °C) need no precious metal at all.
What you need
| Item | For | See |
|---|---|---|
| Platinum wire or foil, 0.3–0.5 mm, a few grams | Grove cell electrodes | Platinum and the Platinum Metals |
| Chloroplatinic acid solution | Platinising (platinum black) | Platinum and the Platinum Metals |
| Glass tubes, beakers, rubber or cork stoppers | Grove cell | Laboratory Glassware |
| Dilute Sulfuric Acid, about 1 part acid to 6 of water | Acid electrolyte | |
| Caustic potash, 25–30% solution | Alkaline electrolyte | Lye and Potash |
| Hydrogen and oxygen, clean and dry; gasholders | Fuel | Hydrogen, Oxygen and Gases |
| Fine nickel powder, carbon black, paraffin wax or other water repellent | Porous electrodes | Nickel and Cobalt, Lampblack and Carbon Black, Powder Metallurgy |
| Graphite blocks or nickel-plated steel plates; rubber gaskets | Stack | Insulators, Cables and Electrical Fittings, Packing, Gaskets and Seals |
| Galvanometer or voltmeter and ammeter | Measuring | Measuring Electricity |
Where to find it
You gather nothing new from nature for a fuel cell; you make its parts from earlier chapters.
- Hydrogen from water by Electrolysis, from iron and acid, or, for large amounts, by passing steam over red-hot coke or Natural Gas and Helium and removing the carbon monoxide (Ammonia describes the gas works). Gas from coke or natural gas carries carbon monoxide, which poisons platinum catalysts at the low-temperature cells; it must be cleaned to a few parts per million, or used only in hot cells.
- Oxygen from electrolysis or from liquid air (Liquid Air, Nitrogen and the Noble Gases). Ordinary air works at the cathode at lower power. For an alkaline cell, the air must first be scrubbed of carbon dioxide by passing it through lime water or a tower of slaked lime (Lime); otherwise the potash slowly turns to carbonate and the cell dies.
- Caustic potash from wood ash and lime (Lye and Potash).
Method 1: Grove's gas battery
This is the first fuel cell, and the best way to see one work. Each cell needs about 10–15 cm of platinum wire or two small strips of foil.
- Electrodes. For each tube, take a strip of platinum foil 1 × 5 cm, or a 25 cm length of 0.3 mm platinum wire wound into a tight, long coil, welded to a lead wire. Platinise it black (Platinum and the Platinum Metals): this alone multiplies the current many times.
- Tubes. Seal each lead wire through the closed end of a glass tube 1.5–2 cm across and 12–15 cm long, so that the strip hangs down inside nearly to the open end (Scientific Glassblowing and Glass-to-Metal Seals). A platinum wire seals straight into soft glass.
- Fill. Fill both tubes with dilute Sulfuric Acid (about 1 part strong acid to 6 of water, poured acid into water) and stand them upside down in a small beaker of the same acid, side by side, about 2–3 cm apart.
- Fill with gas by running it backwards. Connect the two leads to a battery of 3–4 volts for some minutes. Bubbles rise in both tubes: hydrogen at the negative lead, oxygen at the positive, twice as much hydrogen as oxygen by volume. Stop when the hydrogen tube is half full of gas. Now each strip is half in gas and half in acid, and the cell is charged.
- Measure. Disconnect the battery and connect the two leads to a voltmeter. It should read about 0.9–1.0 V, the hydrogen side negative. Connect a sensitive galvanometer or a small current meter: a steady current of a few milliamperes flows (Measuring Electricity).
- Watch it work. As the current runs, the acid slowly rises in both tubes — in the hydrogen tube twice as fast as in the oxygen tube — because the gases are being used up in the same ratio in which electrolysis made them.
A chain. Connect four or five such cells in series (the hydrogen strip of one to the oxygen strip of the next). The 3.5–5 V they give will slowly split water in a small voltameter of two platinum wires in dilute acid, as Grove's 50-cell battery did in 1842. You have made a store of electricity: charge it by electrolysis, discharge it as a fuel cell.
Good versus bad. A good cell holds near 1 V for hours when no current is drawn. If the voltage starts low or falls quickly, oxygen has leaked into the hydrogen tube, the strips are not platinised, or the acid is dirty.
Method 2: The gas diffusion electrode
Grove's strips work only along the thin line where the acid surface meets them. Useful power needs the reaction spread through a porous electrode, with gas filling the pores from behind and liquid wetting their walls from the front. This is the gas diffusion electrode.
Two ways to hold the liquid in place.
- Double porosity (F. T. Bacon's way): a sheet of sintered nickel with coarse pores (about 30 µm) on the gas side and fine pores (about 15 µm) on the liquid side. Capillary force holds liquid in the fine pores; a small gas pressure (a few tenths of an atmosphere) keeps it out of the coarse ones. The meniscus sits at the boundary, inside the metal, over a huge area.
- Wet-proofing: a porous layer of carbon or nickel powder bonded with a water-repelling binder — paraffin wax in early cells, PTFE (a fluorine plastic, Fluorspar and Fluorine Compounds, Petrochemicals and Modern Plastics) later — so the electrolyte wets only part of each pore and gas fills the rest.
Making a wet-proofed carbon electrode
- Catalyst. For hydrogen in alkali: fine nickel powder (Powder Metallurgy), or carbon black coated with platinum black. For oxygen in alkali: carbon black with fine silver (precipitated from silver nitrate with a reducing sugar or formaldehyde, Silver Nitrate and Silver Salts), or platinum black.
- Mix 7 parts of catalyst powder (or catalyst-coated carbon black) with 3 parts of fine paraffin wax dissolved in warm benzine or white spirit (Ether, Acetone and Solvents), into a paste.
- Spread the paste 0.3–0.5 mm thick on a fine nickel gauze (current collector) or on porous carbon paper, and press it in a warm press at 1–2 tonnes per square decimetre.
- Dry and bake gently, around 80–100 °C, so the wax spreads as a thin film through the pores without filling them.
Test: blow gently through the electrode: it should pass air. Drop water on the gas face: it should bead up and stay as drops. Drop it on the catalyst face and it should slowly soak in a little.
Method 3: A small alkaline fuel cell
The alkaline cell, with caustic potash, is the most forgiving: it needs no platinum, and nickel and steel are not attacked by alkali.
- The cell frame. Two gas diffusion electrodes 10 × 10 cm face each other across a gap of 3–5 mm, held in a frame of nickel-plated steel or a stiff plastic, with rubber gaskets sealing their edges (Packing, Gaskets and Seals). The gap is the electrolyte space, with a pipe in at the bottom and out at the top.
- The gas chambers. Behind each electrode, a shallow chamber 2–3 mm deep with ridges to press against it, an inlet and a small outlet. Hydrogen behind one, oxygen (or scrubbed air) behind the other.
- The electrolyte. 25–30% caustic potash in clean water, slowly circulated from a small tank by a pump or by gravity. Circulating it carries away the water made by the cell and the heat. Keep the tank warm, around 60–70 °C, for best output.
- Gas pressure. Feed the gases at a pressure just enough to keep the electrolyte out of the gas chambers — a few centimetres of water on a simple water gauge (Pressure and Vacuum Gauges) — and equal on both sides. Bleed a very small flow from each outlet to carry away any nitrogen or water vapour.
- The stack. One cell gives about 0.7–0.8 V. For a 12 V output, make 16 cells and stack them, the oxygen side of one connected to the hydrogen side of the next. In a neat stack this is done by a bipolar plate of graphite or nickel-plated steel, with gas channels cut in both faces, between each pair of cells; end plates with bolts clamp the whole pile together.
What to expect. A good home-made alkaline cell gives about 50–100 milliamperes per square centimetre at 0.75 V, so a 10 × 10 cm cell gives 5–10 A, about 4–7 W. Sixteen cells make a 12 V, 60–100 W stack: enough to charge batteries or run a radio station. Bacon's high-pressure cells at 200 °C gave several times as much.
The water it makes dilutes the potash. Measure the electrolyte's strength with a hydrometer (The Rechargeable Battery shows how) and evaporate it back when it falls.
Other kinds of fuel cell (outline)
| Type | Electrolyte | Runs at | Catalyst | Notes |
|---|---|---|---|---|
| Alkaline | Caustic potash | 60–200 °C | Nickel, silver, or platinum | Most efficient; killed by carbon dioxide; used on the Apollo and Space Shuttle craft |
| Phosphoric acid | Strong phosphoric acid held in a porous silicon carbide sheet | 150–200 °C | Platinum on carbon black | Tolerates carbon dioxide and a little carbon monoxide; runs on cleaned natural gas; standby power for buildings (Phosphoric Acid and Phosphates) |
| Membrane (proton exchange) | A thin, wet sheet of acid plastic, 0.05–0.2 mm, which carries protons but not gas | 60–90 °C | Platinum on carbon black | Compact, quick to start; for vehicles. Needs very pure hydrogen and a fluorine plastic membrane (Membranes, Reverse Osmosis and Desalination, Water Softening and Ion Exchange, Fluorspar and Fluorine Compounds) |
| Molten carbonate | Molten lithium and potassium carbonate in a ceramic sponge | About 650 °C | Nickel | Burns natural gas or coal gas; for power stations |
| Solid oxide | Dense zirconia ceramic (Zircon and Zirconium) | 700–1,000 °C | Nickel, ceramic oxides | No precious metal; burns natural gas directly; slow to heat up (Rare Earths, Cerium and Phosphors) |
The membrane cell is the one in modern fuel-cell cars and buses. Its membrane is a fluorine-based plastic carrying sulfonic acid groups, like the sulfonated exchangers of Water Softening and Ion Exchange but in a thin, strong film. It must stay damp, so the gases are humidified. Its platinum is spread as particles a few millionths of a millimetre across on carbon black, using a fraction of a milligram per square centimetre; early cells needed tens of times more.
How to tell it worked
- Open-circuit voltage about 1.0 V per cell (0.9–1.05), steady for hours.
- Gas use matches current: 0.45 litres of hydrogen per ampere-hour. If the cell uses much more, gas is leaking or crossing over.
- Water appears: in the acid cell at the oxygen side, in the alkaline cell at the hydrogen side; collect and weigh it, 0.34 g per ampere-hour.
- Load test: draw increasing current and plot the voltage. A healthy cell holds above 0.7 V at its rated current.
Note Troubleshooting. Voltage low with no load (below 0.8 V) → gases mixing through a leak or a cracked electrode, or catalyst poisoned. Check seals; replatinise. Voltage falls quickly under load → too little catalyst surface, electrodes flooded with electrolyte, or gas starved. Raise the gas pressure slightly, improve wet-proofing, platinise more. Liquid bubbling into a gas chamber → gas pressure too low, or electrode pores too big. Raise the pressure. Gas bubbling through into the electrolyte → gas pressure too high. Lower it. Alkaline cell slowly weakens over days, white crust → carbon dioxide has turned the potash to carbonate. Scrub the air better; renew the electrolyte. Platinum cell dies on gas from coke or natural gas → carbon monoxide poisoning. Clean the gas, or use electrolytic hydrogen.
Dangers
Danger Hydrogen and oxygen together explode. A fuel cell keeps them apart by a few millimetres of wet porous material. A cracked electrode or a dry membrane lets them mix, and a platinum catalyst can light the mixture by itself. Never store the two gases near each other; put flame arresters (fine wire gauze in the pipe) and non-return valves in both gas lines; never run a cell with a leaking seal; work where any leak can rise away freely (Hydrogen, Oxygen and Gases).
Danger Caustic potash burns skin and blinds eyes, and hot potash worse. Wear eye protection and gloves, and keep plenty of clean water at hand. Wash a skin splash with running water for at least 20 minutes; an eye splash for at least 30 minutes, holding the lids open. Never put vinegar in an eye (Lye and Potash).
- Pure oxygen makes oil, grease, cloth and rubber burn fiercely. No oil on oxygen fittings.
- Carbon monoxide in reformed gas from coke or natural gas is a silent poison. Vent it outdoors (Natural Gas and Helium).
- Electrical: a large stack can deliver hundreds of amperes into a short circuit. Fuse it.
- Chloroplatinic acid and platinum salts cause a lasting allergy (Platinum and the Platinum Metals).
What this unlocks
Long-lasting, silent electric power in spacecraft (Spaceflight and Spacecraft) and submarines; standby power for radio and telephone stations (Radio, The Automatic Telephone Exchange); fuel-cell vehicles (Electric Vehicles); seasonal storage of surplus wind and water power as hydrogen (Storing Energy, Wind Turbines). Small cells of the same kind make the oxygen sensors of Medical Oxygen supplies and car engines, and the breath-alcohol testers of police, and the reverse machine — a membrane electrolyser — splits water more efficiently than the old diaphragm cells (Electrolysis).
How it was first done
In January 1839 the Swiss–German chemist Christian Friedrich Schönbein reported that platinum in hydrogen and oxygen gave a current. That same year the Welsh lawyer and scientist William Robert Grove wrote of a cell of two platinum strips in dilute acid, one in hydrogen and one in oxygen. In 1842 he described his "gas voltaic battery" of 50 cells, which split water, and he understood that the reaction happened only where gas, liquid and platinum met. In 1889 Ludwig Mond and Carl Langer in England used porous platinum-black electrodes on a soaked earthenware sheet, ran them on coal gas, and named the device a fuel cell.
The cell became practical through the patient work of the English engineer Francis Thomas Bacon, who from 1932 to 1959 developed an alkaline cell with porous nickel electrodes; in 1959 he showed a 5 kW stack. Pratt & Whitney built Bacon-type alkaline cells for the Apollo spacecraft (1960s), which made the electricity and drinking water for the flights to the Moon. Meanwhile Thomas Grubb and Leonard Niedrach at General Electric made the first membrane cells, flown in the Gemini spacecraft from 1965. Phosphoric acid cells went into buildings in the 1990s, and membrane fuel-cell cars and buses were sold from the 2010s.
Source: content/entries/electricity/fuel-cells.md