◆ Rebuild

Part 2 · Earth and Fire

Stoneware and Porcelain

Fired hot enough — 1,250–1,300 °C — the right clays melt partly into glass and become stoneware and porcelain — hard, dense, waterproof even without glaze, and resistant to almost every acid. This chapter covers finding the clays, mixing a porcelain body of kaolin, feldspar and quartz, and building the downdraft or climbing kiln that reaches the heat.

Difficulty
●●●●●
Time
Months to find and test clays and build the kiln; one to two days per firing and two days to cool
Steps from zero
10 prerequisites →

You need first

The KilnGlazesFirebrick and Refractories

This unlocks

Toilets, Sinks, Baths and ShowersInsulators, Cables and Electrical FittingsPiezoelectric Crystals and Ceramics
The full path from nothing — 10 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. The Kiln
  4. Pottery
  5. Lime
  6. Bricks
  7. Lye and Potash
  8. Glass
  9. Firebrick and Refractories
  10. Glazes
  11. Stoneware and Porcelain

Do them roughly in this order. See it on the tech tree →

Why it matters

Ordinary earthenware (see Pottery) is fired at 900–1,100 °C. It stays porous, soaks up liquid, and is easily chipped. Take the right clay to 1,250–1,300 °C and it changes: part of it melts into glass that fills every pore. The result is stoneware — or, from very pure white materials, porcelain. These are:

This chapter is hard. Building a kiln that reaches 1,300 °C and finding the right clays will take many attempts. Aim for stoneware first. Porcelain is the same craft with purer materials and less room for error.

How it works

Vitrification means "turning to glass". As a clay body heats past about 1,100 °C:

  1. The fluxes in it — potash and soda (mostly from feldspar and mica), lime, iron — begin to melt into a sticky glass.
  2. The glass flows into the pores and pulls the grains together. The body shrinks (12–15% from wet to fired) and becomes dense.
  3. Long needle-shaped crystals of mullite (an aluminium silicate) grow from the clay and lock the body together like the fibres in felt.
  4. Unmelted quartz grains stay as a skeleton that keeps the pot from slumping.

Too little heat and the pores stay open. Too much and the glass takes over: the pot softens, slumps, warps, and gas bubbles blow it up like bread (bloating). Stoneware has a firing window of perhaps 30–60 °C. That is why good thermometry — draw trials and cones — matters here more than anywhere else.

Ware Firing heat Water absorbed (by weight) Look
Earthenware 900–1,100 °C 5–15% Porous, sticks to the tongue
Stoneware 1,200–1,300 °C 0.5–3% Dense, grey, buff or brown; rings like a bell
Porcelain 1,250–1,400 °C Under 0.5% White, glassy, thin pieces glow when held to light
Earthenware900–1,100 °C: grains touch,open pores between them Stoneware1,200–1,300 °C: melted glassfills most pores Porcelain1,280–1,400 °C: glass, mulliteneedles, a few quartz grains Magnified view of a broken edge. Pale round grains: quartz.
Fig. 1 How a clay body changes with heat. Earthenware is grains with open pores; in stoneware, melted glass fills most pores; in porcelain, glass, mullite needles and quartz form an almost solid mass.

What you need

Item Notes
A stoneware clay, or materials to blend one See below
For porcelain: kaolin, feldspar, quartz Washed and ground very fine
A high-temperature kiln Downdraft or climbing kiln of firebrick; see below and Firebrick and Refractories
Firebricks 1,000–3,000 for a small kiln
Kiln furniture Fireclay shelves, posts and saggars (lidded fireclay boxes)
Firewood 2–5 m³ of very dry, split softwood per firing for a small kiln; pine is best for the final climb
Grinding gear Quern or stamp mill, sieves of fine cloth, settling tubs (see Abrasives and Grinding Stones)
A balance For weighing recipes and absorption tests (see Measurement from Scratch)

Where to find it

  • Stoneware clays are common. Many grey or buff fireclays and pale sedimentary clays — the kind found under coal seams and in old lake beds — vitrify at 1,250–1,300 °C because they contain a little natural flux. See Firebrick and Refractories for finding and testing them.
  • Kaolin (china clay) forms where granite has rotted in place. Look for white, chalky patches in granite country, full of loose quartz grains and glittering mica. Wash it: stir in water, let the sand and mica sink for a minute, pour off the milky water, and let the kaolin settle for a day.
  • Feldspar is the second-commonest mineral in granite: blocky crystals, white, cream, pink or grey, with flat shining cleavage faces. It is softer than quartz (a steel knife barely marks it and a file scratches it; neither scratches quartz). Coarse granites called pegmatites have feldspar crystals as big as a fist. Rotted granite with half-weathered feldspar — the Chinese "petuntse" or English "china stone" — is a ready-made porcelain flux.
  • Quartz — white vein quartz or clean quartz sand. Heat lumps red-hot and drop them in water to make them crumble.

Finding or making a stoneware body

  1. Test every pale clay by firing small bars and cups to the highest heat your kiln reaches.
  2. The absorption test. Weigh a fired piece dry, boil it in water for an hour (or soak it for a day), wipe the surface and weigh it again. The gain divided by the dry weight is its absorption. Below 3% is stoneware.
  3. Without a balance: touch the fired piece to your tongue — earthenware sticks; stoneware does not. Put a drop of Ink on an unglazed broken edge, wait a minute and wipe it: on stoneware the ink wipes off almost completely; on earthenware it soaks in.
  4. Blend if needed. If a clay is too refractory (still porous at your top heat), mix in a more fluxing clay — even 10–30% of a red earthenware clay — or 10–20% ground feldspar. If it slumps or bloats, add fireclay, kaolin or fine quartz. Test each blend, and write it down.
  5. Add fine grog (10–20%) to large pieces and kiln-ware to reduce cracking.

Porcelain body

A good starting recipe, by dry weight:

Ingredient Parts Job
Kaolin 50 Gives whiteness, alumina and mullite
Feldspar 25 The flux that melts into glass
Quartz 25 The skeleton; also helps the glaze fit
  1. Grind the feldspar and quartz until they pass the finest cloth you have and feel smooth, not gritty, between your teeth. Grind them wet; this is long, hard work (a water-powered stamp mill or ball mill helps — see The Waterwheel).
  2. Mix all three in water to a thin cream, sieve again, and let it thicken by settling and pouring off water, then on plaster or dry clay slabs.
  3. Age it. Kaolin is not very sticky. Store the wet body covered for weeks or months — Chinese potters aged porcelain clay for years. Wedge it well before use (see Finding and Preparing Clay). Adding 5–10% of a fine, plastic pale clay makes it easier to throw on the The Potter's Wheel. Thin, even porcelain is also cast from liquid body in plaster moulds (Slip Casting, Jiggering and Ceramic Factories).
  4. Shape it thinly: 3–5 mm walls for tableware. Porcelain warps easily; keep shapes simple and even.
  5. Dry slowly and evenly.
  6. Bisque at 800–900 °C, glaze (see below), then fire to 1,280–1,320 °C.

Glazes for high heat

At stoneware heat the simplest glazes work (see Glazes):

  • Ash glaze: 1 part washed wood ash to 1 part clay.
  • Feldspar glaze: 40 feldspar, 30 quartz, 20 ground limestone, 10 kaolin, by weight. Clear and glossy on porcelain at about 1,280 °C.
  • Celadon: the same with 1–2% iron, fired in a smoky (reduction) fire — the pale jade-green of Chinese and Korean ware.
  • Salt glaze — salt thrown into the firebox at full heat (see Glazes).

On porcelain, glaze and body mature together in one firing, and fuse at the boundary so tightly they cannot be separated.

Building a kiln that reaches 1,300 °C

A simple updraft The Kiln tops out at about 1,100–1,150 °C: the heat passes straight through the pots and out of the top. To go higher you need firebrick (Firebrick and Refractories), a long flame path, and a strong chimney draught. Two proven designs:

The downdraft kiln

Firebrick arch, 23 cm thick Bag wallthrows flame upward Firebox and grateair and wood enter at the stoke hole Exit holes in the floorinto a channel to the chimney Chimneyabout 3 × chamber height Dampersliding brick Ware on shelvesor in saggars
Fig. 2 A downdraft kiln. Flames rise from the firebox behind a low bag wall, sweep up to the arched roof, are pulled down through the ware to exit holes in the floor, and leave through a tall chimney. The heat passes the pots twice.
  • Chamber: about 1 m wide, 1 m deep and 1.2 m high to the top of an arched roof, built of firebrick 23 cm thick (one brick length), with an outer skin of ordinary brick or earth for insulation.
  • Firebox: along one or both sides, with a stoke hole and a grate of firebrick bars or iron bars, and an ash pit below for air.
  • Bag wall: a low wall of loosely laid firebricks between the firebox and the ware, 40–60 cm high, that throws the flames upward.
  • Exit flues: a row of holes along the floor on the side opposite the firebox, leading into a channel under the floor to the chimney.
  • Chimney: tall — roughly 3 times the height of the chamber, so 4–5 m — with an inside cross-section about the same as the total area of the exit flues (about 20 × 20 cm for a small kiln). A sliding brick damper in the chimney controls the draught.

Because the flame goes up, turns, and is pulled down through the ware, the whole chamber heats evenly, and the heat stays longer inside.

The climbing kiln

Main fireboxfired first Side stoke holeseach chamber fired in turn Hot gas from belowpreheats the next chamber Chambers step up the hillthe slope acts as a chimney Short flue slope 15–20°
Fig. 3 A climbing kiln on a hillside. Each chamber is fired in turn through side stoke holes; the hot gas from one chamber preheats the next, and the slope itself acts as a chimney.

Chinese and Japanese potters built kilns up a hillside slope of 15–20°. The simplest is a single long tunnel (the Japanese anagama, the Chinese "dragon kiln"); later ones were a row of chambers, each a little higher than the last. The slope works as a chimney. You fire the firebox at the bottom first, then stoke each chamber through holes in its sides in turn. Hot gas from below preheats the chambers above, so the kiln uses its fuel very efficiently. A climbing kiln needs a suitable slope and a lot of building, but no tall chimney.

Step by step: a stoneware firing

  1. Load the ware on fireclay shelves and posts. Paint shelves with a wash of kaolin and quartz (equal parts in water) so glaze drips do not stick. Put porcelain and white ware in saggars to protect them from flying ash. Place draw trials (small glazed rings) and, if you have them, cones (see Pyrometric Cones and Kiln Temperature) where you can see them through spy holes.
  2. Water-smoke slowly: a small fire for 4–8 hours until no moisture fogs a cold stone held at the chimney.
  3. Climb steadily, about 100 °C per hour, stoking small amounts often. Go especially gently through 573 °C (dull red).
  4. Above 1,000 °C (orange) the kiln will slow down. Stoke split, very dry softwood in small handfuls, every few minutes, as soon as the flame at the chimney shrinks. Expect the last 200 °C to take as long as everything before.
  5. Reduction (for celadon or iron glazes): from about 1,000 °C, partly close the damper so a little smoky flame shows at the spy holes and chimney. Keep it moderate — heavy smoke stalls the temperature. For clear colours in clean, airy fire, keep the damper open.
  6. Top temperature: yellow-white, too bright to look at long; ware and walls glowing the same colour with no shadows (see The Kiln). Pull draw trials: when the glaze is fully glossy and a broken trial looks glassy, not chalky, inside, hold the heat for one to two hours.
  7. Close up: stop stoking, close stoke holes, ash pit and damper, and seal them with mud.
  8. Cool slowly — at least 24–48 hours for a small kiln. Stoneware is especially prone to cracking (dunting) as it cools through 573 °C and again at about 220 °C. Do not open the kiln until you can hold your hand on the door bricks.

A small downdraft firing takes 16–30 hours and many cubic metres of wood. Work in shifts.

How to tell it worked

  • The ware rings clearly and is very hard: a steel knife leaves only a grey metal streak, no scratch.
  • Absorption below 3% (stoneware) or 0.5% (porcelain). Unglazed bases do not stick to the tongue or soak up ink.
  • Porcelain is white, and a thin piece glows warmly when held up to the sun or a lamp.
  • Acid test: fill a piece with strong vinegar for a week; it should not lose weight, shine or strength.
  • A broken edge looks smooth and glassy, like stone, not grainy like brick.

Note Troubleshooting. Still porous → underfired, or the body is too refractory: fire longer and hotter, or add feldspar or a fluxing clay. Blisters and swollen, bloated pieces → overfired, or iron-rich clay fired in heavy reduction: lower the top heat, reduce less. Slumped and warped → too hot, too much flux, or poor support; add kaolin or quartz, set pieces on flat shelves, fire a little cooler. Sharp, clean cracks found on opening (dunting) → cooled too fast; seal the kiln better and wait longer. Black core in a broken piece → carbon trapped by reduction that started too early: keep the fire clean and airy until 1,000 °C. Kiln stalls at yellow-orange → wet or thick wood, ash choking the grate, too short a chimney, or leaks letting cold air in. Glaze crazes → add quartz to the glaze (see Glazes).

Dangers

Danger Extreme heat. A kiln at 1,300 °C radiates enough heat to burn skin a metre from a spy hole, and the chimney and roof are hot enough to ignite wood and thatch. Build well away from buildings and trees, wear wool or leather (never anything that melts), and keep water and sand ready.

Danger Silica dust. Grinding quartz, feldspar, kaolin and grog is the most dangerous part of ceramics. The fine dust scars the lungs for life (silicosis). Grind wet, sweep wet, work outdoors, and cover your nose and mouth with a damp cloth.

  • Eyes. Looking into a white-hot kiln, firing after firing, causes cataracts over years. Look briefly, through a piece of dark glass if you have one, and never stare.
  • Carbon monoxide pours from a kiln in reduction. Never fire in a closed shed, and keep the area around the kiln ventilated.
  • Collapse. Arches and chimneys weaken with every firing. Check them and rebuild before they fall.
  • Exhaustion. Long firings cause mistakes. Work in shifts, and never alone.

What this unlocks

Stoneware gives safe storage for food, drink and chemicals (Preserving Food, Fermentation, Acids, Bases and Testing); acid-proof vessels for Sulfuric Acid, Nitric Acid and Electrolysis; and vitrified Tiles and Clay Pipes for Sewers and Wastewater and Pipes, Plumbing and Aqueducts. Porcelain gives crucibles and dishes for chemistry (Laboratory Glassware), and insulators for the The Telegraph, Power Lines and Distribution and the The Internal Combustion Engine engine's spark plug. The same kilns, fuel and skills feed Portland Cement and better Glass.

How it was first done

Chinese potters were the first to reach stoneware heat, firing glazed stoneware during the Shang dynasty more than 3,000 years ago; the first long kilns built up hillsides appear in south China at about the same time. By the Eastern Han dynasty (about the 2nd century AD), kilns in what is now Zhejiang were making near-porcelain with green celadon glazes, and by the Tang dynasty (7th–10th centuries) Chinese potters made fine white porcelain. Jingdezhen, rich in kaolin and porcelain stone, became the porcelain capital of the world, with dragon kilns tens of metres long. Korean and Japanese potters developed their own climbing kilns. Europeans tried for centuries to copy porcelain; potters in the Rhineland made strong stoneware from about the 14th century and salt-glazed it from around 1400, but true hard porcelain was first made in Europe only in 1708–1709 at Dresden by Ehrenfried Walther von Tschirnhaus and Johann Friedrich Böttger, leading to the Meissen factory. In England, William Cookworthy made porcelain from Cornish china clay and china stone in 1768. In the 19th century, chemical stoneware for acids and the porcelain insulator made ceramics a pillar of the chemical and electrical industries.

Source: content/entries/earth/stoneware-and-porcelain.md