Part 8 · Chemistry
Sulfur
Sulfur — the yellow "brimstone" of volcanoes — can be picked up, melted out of rock at a little above the boiling point of water, or driven out of pyrite by heat. It is the key to sulfuric acid, the most important chemical of industry.
- Difficulty
- ●●●●●
- Time
- Hours to gather and melt; days to weeks for a calcarone burn
- Steps from zero
- 0 prerequisites →
You need first
Nothing — start here.Why it matters
Sulfur is a yellow, brittle, light stone that melts like wax and burns with a blue flame. For thousands of years people called it brimstone — "burning stone". It is one of the few chemical elements that you can find lying on the ground almost pure.
With it you can:
- make Sulfuric Acid, the chemical that opens the way to batteries, fertiliser and almost every other acid — this is by far its most important use;
- dip wooden splints in it to make sulfur matches that catch fire from a single glowing ember (Matches);
- fumigate barrels, granaries and clothing against mould, insects and lice — and keep wine from spoiling (Fermentation);
- dust it on grapevines and crops against mildew and other fungus diseases (Farming from Seed);
- treat scabies and other skin parasites with sulfur ointment (Personal Hygiene);
- later, harden natural rubber (vulcanisation, Rubber) and make many other chemicals.
It was also one of the three ingredients of gunpowder, which is covered for its history in Black Powder (history).
How it works
Sulfur is an element — a basic substance that cannot be split into anything simpler. Deep underground, volcanic heat drives sulfur out of rocks as gases: hydrogen sulfide (which smells of rotten eggs) and sulfur dioxide (the choking smell of a struck match). Where these gases reach the surface and cool, or react with each other, they leave crusts of pure yellow sulfur. Other deposits formed in ancient seabeds, where bacteria turned gypsum into sulfur among layers of limestone.
Sulfur has three properties that make it easy to win from rock:
- It melts at only about 115 °C — a little hotter than boiling water — while the rock around it doesn't melt at all. Heat crushed sulfur ore gently and the sulfur simply runs out. This is called liquation.
- It boils at about 445 °C and turns into a vapour that condenses back into yellow powder or liquid on anything cool. So you can distil it, from ore or from pyrite.
- It burns at about 250 °C. If you heat it too hot in air, it catches fire and is lost as choking gas. This can be turned to advantage: in the Sicilian calcarone, part of the sulfur is deliberately burned to provide the heat that melts the rest.
Sulfur is its own thermometer. Watch its colour as it melts:
| What you see | Temperature | Meaning |
|---|---|---|
| Pale yellow, brittle solid | Below 115 °C | Not melted |
| Clear, runny, straw-yellow to amber liquid | 120–155 °C | Perfect — pour and work it here |
| Dark red-brown, thick as treacle, won't pour | Above about 160 °C | Too hot. Reduce the heat |
| Blue flame, choking white fumes | Over 250 °C, in air | Burning. Smother it with a lid |
What you need
| Item | Details |
|---|---|
| Sulfur ore | Native sulfur crusts, or rock with yellow veins and crystals; or pyrite |
| Hammer stone | For breaking ore into walnut-sized pieces |
| Two clay pots | For the two-pot melt: one with 6–10 holes (each 5–8 mm) in its base, one to catch |
| Fuel | Wood or charcoal (Charcoal); only gentle heat is needed |
| Moulds | Wooden troughs or clay moulds, wetted with water so the sulfur doesn't stick |
| Lid | A clay lid or flat stone to smother any flame |
| Water | A full bucket, for burns and to cool moulds |
Where to find it
- Volcanic vents (fumaroles and solfataras). Steaming cracks and vents in active and dormant volcanic areas — Iceland, Italy, Japan, Indonesia, the Andes, Kamchatka, New Zealand, the western United States and many others. Look for bright lemon-yellow crusts, needles and crystals around vents, often mixed with white and orange deposits and bubbling grey mud. The air smells of rotten eggs or burnt matches. Some vents have built up masses of nearly pure sulfur many metres thick.
- Hot springs that smell of rotten eggs often coat their channels with yellow-white sulfur and white, slimy deposits.
- Sedimentary sulfur. In some dry regions — famously Sicily, also parts of Poland, Iraq, Texas and Louisiana — yellow sulfur forms veins and nodules in grey limestone, marl and gypsum (a soft white rock you can scratch with a fingernail). Ore with 20–30 % sulfur is rich.
- Pyrite (iron sulfide, "fool's gold") is far more widespread: brassy cubes and lumps in shale, slate, coal seams and ore veins. It is more than half sulfur by weight. See Finding and Identifying Ores.
How to recognise native sulfur:
- Bright lemon to pale yellow, with a greasy or resin-like shine. Older surfaces may be dull or greenish-yellow.
- Soft: a fingernail barely scratches it, and a knife cuts it easily. It is brittle and crumbles.
- Light for a stone — about twice the weight of the same volume of water; ordinary rock is two and a half to three times.
- Hold a clean crystal in a warm hand close to your ear: it may crackle faintly as the warmth makes it crack.
- The decisive test: touch a tiny chip to an ember. It melts into a reddish-brown drop, burns with a small blue flame, and gives off the sharp, choking smell of a struck match. Nothing else common looks yellow and does this.
Method 1: Hand-picking and simple melting
Volcanic sulfur crusts are often 80–99 % pure. Knock them off with a stick (keep your face away from the vent), pick out the cleanest yellow pieces, and simply melt them gently in a clay pot over low embers. Stir; the sulfur melts to a clear amber liquid while sand and rock sink. Ladle the clear liquid off the top into wetted moulds.
Method 2: The two-pot melt (liquation)
This is the best small-scale method for poorer ore.
- Dig in the catch pot. Bury a clay pot in the ground up to its rim. It stays cool, so the sulfur sets as it arrives.
- Place the ore pot. Stand the pot with holes in its base on top, its base resting in the mouth of the buried pot. Seal the joint around the outside with wet clay so ash and fire stay out.
- Fill it with ore broken to walnut size. Cover the top with a clay lid sealed with clay — air must be kept out, or the sulfur will burn.
- Build a fire around the upper pot only. Keep it gentle. You want the pot hot enough that a drop of water spat on its side sizzles and dances away, but no visible glow. Too hot and the sulfur turns thick and dark and starts to burn; too cool and nothing runs.
- Wait. After about an hour, molten sulfur starts dripping through the holes. Keep the fire steady for another 2–3 hours, depending on the size of the pots.
- Let everything cool, lift off the upper pot, and empty the spent rock. Break the cake of yellow sulfur out of the lower pot.
- Re-melt and pour. Melt the cake gently in a clean pot, skim off any scum, and pour the clear liquid into wetted moulds as sticks or blocks. Pure sulfur sets bright yellow.
With ore of 20–30 % sulfur, expect to recover roughly half to two-thirds of it this way. The spent rock still contains sulfur and can go into a calcarone.
Method 3: The calcarone
For larger amounts, Sicilian miners from the 1850s onwards used the calcarone: a pile of ore that melts itself. About a third of the sulfur burns, and its heat melts the rest.
- Choose the site on a hillside, far downwind of homes, crops and water — the smoke kills plants for hundreds of metres.
- Build the floor. Make a round, shallow pit 3–10 m across, with a hard-packed clay or stone floor that slopes down to one point at the front of the pit, at about 1 in 6. Build a low circular wall of stones and clay around it, with a small tap hole at the lowest point, closed with a clay plug.
- Stack the ore. Lay the biggest lumps at the bottom, leaving channels for air, and pile smaller ore on top into a dome. Build in a few vertical channels for lighting and draught.
- Cap it. Cover the whole heap with 10–20 cm of spent ore (the burnt-out rock from earlier burns) or earth. This slows the burn and keeps out too much air.
- Light it from the top, through the channels, with burning brushwood. The fire creeps slowly downwards through the heap over days to weeks, depending on the size. Close or open the vents to keep it smouldering, never blazing: you should see thin wisps of white smoke, not flames.
- Tap it. Every day or two, open the tap hole. Molten sulfur runs out like amber syrup into wetted wooden moulds. Close the hole again with clay.
- When no more runs, let it cool and dig out the spent ore for capping the next burn.
A well-run calcarone recovers about two-thirds of the sulfur in the ore. The rest goes up as sulfur dioxide. Later Sicilian furnaces with several chambers (the Gill furnace of 1880) used the hot gas from one chamber to preheat the next and lost much less.
Method 4: Sulfur from pyrite
If you have no volcanoes or sulfur beds, pyrite is your source. Heated strongly without air, pyrite gives up part of its sulfur as vapour, leaving a dark, crumbly iron sulfide behind.
- Crush pyrite to pea size and fill a clay retort or a thick clay tube closed at one end — the same kind of vessel as the green-vitriol retort in Sulfuric Acid. Lead its open end, sloping down, into a pot half-filled with water.
- Heat the retort to bright red (about 700–800 °C) in a The Kiln or charcoal fire with a Bellows.
- Sulfur vapour distils over and condenses in the cool water as yellow lumps and drops. Collect and re-melt them.
- In theory, pyrite can give a quarter of its weight in sulfur this way; in practice, expect perhaps a tenth to a fifth.
Pyrite can also simply be roasted in air. Then its sulfur burns to sulfur dioxide gas instead — useless as sulfur, but exactly what you want if your aim is Sulfuric Acid.
How to tell it worked
- Colour and feel: bright yellow, light, brittle, snaps cleanly. Brownish or greyish sulfur holds dirt or iron; re-melt it, let the dirt settle, and pour off the clear top.
- The burn test: a small piece should burn away almost completely with a blue flame, leaving almost no ash. A lot of grey ash means rock is mixed in.
- The melt test: good sulfur melts to a clear amber liquid with nothing gritty at the bottom.
Note Troubleshooting. Nothing drips from the two-pot melt → too cool, or the holes are blocked by fine ore. Use larger lumps; build up the fire a little. Thick, dark, tarry sulfur → overheated. Let it cool to straw-yellow liquid before pouring. Blue flames and choking smoke → air is getting in and the sulfur is burning. Smother with the lid; seal joints with clay. Calcarone burns out fast with little yield → too much air. Thicken the cap, close vents. Calcarone goes cold → too little air. Open a vent at the top.
Dangers
Danger Volcanic gases kill. Hydrogen sulfide smells of rotten eggs at low levels, but at high levels it paralyses your sense of smell and then your breathing within minutes — so a smell that suddenly vanishes is a warning, not relief. Carbon dioxide has no smell at all and pools in hollows and craters. Never go down into a hollow, pit or crater near vents; stay upwind; work in pairs; leave immediately if you feel dizzy, get a headache, or your eyes burn. Ground near vents may be a thin crust over boiling mud or acid water — test it with a stick before every step.
Danger Burning sulfur makes sulfur dioxide. It attacks the eyes, throat and lungs, can trigger fatal attacks of asthma, and in an enclosed space can kill. Melt and burn sulfur only outdoors, standing upwind. Fumigate rooms and barrels only when nobody is inside, then air them for many hours.
- Molten sulfur burns. It sticks to skin like hot wax at 120–150 °C. Cool the burn in water for 20 minutes; do not peel the sulfur off — it will come away as the skin heals. See Wound Care and Antiseptics.
- Sulfur fires. Burning sulfur flows like a burning liquid, and its blue flame is hard to see in daylight. Smother it with a lid, sand or earth.
- Dust explodes. Fine sulfur dust in the air can explode when it meets a flame. Grind it in small amounts, outdoors, away from fire.
- Never mix sulfur with saltpeter, chlorates or other strong oxidisers for storage. The mixtures burn violently. Store sulfur separately.
- Pollution. The smoke from roasting and calcaroni destroys crops, kills trees and makes acid rain. Site this work far from fields and water sources.
What this unlocks
- Sulfuric Acid — the most important use by far.
- Fermentation — sulfur fumes keep barrels clean and wine from spoiling.
- Farming from Seed — sulfur dust and lime-sulfur sprays against fungus diseases.
- Medicinal Plants and Personal Hygiene — sulfur ointment (1 part finely ground sulfur to 9 parts fat by weight, half that strength for babies and small children) rubbed on the whole body for three nights is an old and effective treatment for scabies.
- Black Powder (history) — its historical role, and why sulfur was a strategic material for centuries.
- Rubber — heated with natural rubber, sulfur makes it tough and elastic (vulcanisation, discovered by Charles Goodyear in 1839); synthetic rubbers are cured the same way (Synthetic Rubber Works (Overview)).
How it was first done
Sulfur has been known since prehistory because it lies on the ground in volcanic lands and burns so strikingly. In Homer's Odyssey, written down around the 8th century BC, Odysseus purifies his hall with burning sulfur. The Romans used it to bleach cloth, fumigate houses and make medicines, and Pliny the Elder describes sulfur from the volcanic islands near Sicily.
Sicily dominated the world's sulfur supply through the 1800s, when demand for sulfuric acid exploded. Its mines were notorious: much of the ore was carried up from the pits by boys called carusi. In 1840 a quarrel over the Sicilian sulfur trade even brought Britain and the Kingdom of the Two Sicilies close to war. The calcarone was introduced in the 1850s, and the more efficient Gill furnace in 1880. In the 1890s Herman Frasch in Louisiana learned to melt sulfur deep underground with superheated water and pump it up, and Sicily's dominance ended. Today most sulfur is a by-product of cleaning natural gas and oil.
Source: content/entries/chemistry/sulfur.md