◆ Rebuild

Part 9 · Health and Medicine

Dental Instruments and Fillings

How to make the dentist's kit from steel and glass — mouth mirror, probes, scalers, excavators, elevators and extraction forceps, the treadle dental drill and its burrs — how to fill a tooth with zinc oxide–eugenol or zinc phosphate cement, what amalgam and glass ionomer are, and how to keep every instrument sterile.

Difficulty
●●●●●
Time
An afternoon for a probe or scaler; two days for a pair of forceps; two to four weeks for a treadle dental engine; 20–40 minutes to place a filling
Steps from zero
19 prerequisites →

You need first

DentistrySteel

This unlocks

—
The full path from nothing — 19 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sanitation and Germs
  7. Hunting and Trapping
  8. Basic Woodworking
  9. Pottery
  10. Charcoal
  11. Hides and Leather
  12. Fermentation
  13. Bellows
  14. Distillation
  15. Iron (the Bloomery)
  16. Sterilising Instruments and Dressings
  17. Blacksmithing
  18. Dentistry
  19. Steel
  20. Dental Instruments and Fillings

Do them roughly in this order. See it on the tech tree →

Why it matters

Dentistry teaches what to do: keep teeth clean, pull a hopeless tooth, plug a hole. This chapter is about the tools. Bad tools cause most of the harm in rough dentistry: a blunt elevator slips and stabs the palate, forceps with the wrong beaks crush the crown and leave the root, a filling over half-cleaned decay falls out within a month. The difference between pulling every aching tooth and saving most of them is a small drill, a few sharp spoons and a cement that sets hard in the mouth.

How it works

Every dental instrument is a handle, a shank and a working end. The handle is held like a pen, 8–10 mm thick and ridged so wet fingers don't slip. The shank is bent so the working end reaches the back teeth while the hand stays outside the mouth. The working end is tiny: a point, blade or spoon 1–3 mm across.

Three rules hold for all of them:

  1. One piece, smooth all over. Blood dries into cracks, and germs in dried blood survive boiling. Forge from a single bar where you can, and polish.
  2. The right hardness. Cutting tips (scalers, excavators, burrs) are tempered hard to keep an edge. Levers and forceps are tempered softer so they bend rather than snap in the mouth. Tempering colours are in Steel.
  3. A finger rest. One finger of the working hand always rests on a nearby tooth, so a slip stops within a centimetre.

What you need

Item Use Made from
High-carbon steel bar and wire, 3–12 mm All instruments Steel; old files and springs (Files and Saws)
Forge, small anvil, hammers, tongs Shaping Blacksmithing
Needle files, fine whetstones, polishing powders Finishing Files and Saws, Abrasives and Grinding Stones
Small lathe or bow-turned "turns" Burrs, handles, drill spindle The Lathe, Watches and Small Clocks
Silvered glass or speculum metal Mirror faces Mirrors
Zinc oxide; clove oil Fillings, dressings Zinc and Brass, Distillation
Phosphoric acid Zinc phosphate cement Phosphoric Acid and Phosphates
Thick glass slab, steel spatula Mixing cement Glass
Autoclave or boiling pot, cloth packs Sterilising Sterilising Instruments and Dressings

Where to find it

  • Steel of about 0.8–1 % carbon (files, springs, razors) hardens fully and holds an edge; mild steel and wrought iron do not. The spark test is in Steel.
  • Zinc oxide is the fluffy white smoke of burning zinc (Zinc and Brass). Test: yellow when hot, white when cold. Clove oil is steam-distilled from dried cloves (Distillation); good oil numbs the tongue.
  • Handles can be boxwood or bone (Horn and Bone Working), but all-steel instruments survive the autoclave far longer.

The examining set

Mouth mirrorface 20–24 mm across Sharp probeneedle point, crook-shaped Gum probeball tip; rings at 3.5, 5.5 mm Sickle scalertriangular blade, two edges Excavatorsharp spoon 1–2 mm across Straight elevatorhollow blade 3–5 mm wide Pluggerflat end 1–2 mm, packs filling handles 12–13 cm long, 8–9 mm thick, ridged for grip working ends enlarged
Fig. 1 The hand instruments of a basic dental kit, with the working ends enlarged. Every working end is small, smooth and sits on a bent shank so it reaches the back teeth while the fingers stay outside the mouth.

Mouth mirror

A small round mirror that shows the hidden sides of teeth, holds back cheek and tongue, and throws light into the mouth.

  • Face: a disc 20–24 mm across. Best is a front-surface mirror of polished speculum metal (two parts copper to one of tin, Bronze) or glass silvered on the front (Mirrors). Back-silvered glass works but shows a faint double image.
  • Cup and stem: a shallow brass cup with its rim turned over the disc and sealed with shellac, soldered (Soldering and Brazing) to a stem 4–5 cm long, slightly bent. The stem screws into a handle 12–13 cm long, so one handle takes many heads; heads scratch and wear out.

Good: a sharp single image, no rust under the rim. Warm it in the hand or wipe it with a film of soap and it will not fog.

Dental probes

  • Sharp probe (explorer): steel wire 1.5–2 mm, filed to a long taper and a needle point, bent like a shepherd's crook so the tip meets the tooth from above. Harden; temper brown to purple (about 260–280 °C) so it is stiff but springy. Draw it lightly along filling edges and stained grooves: soft decay feels leathery and catches. Never jab pits; it breaks weakened enamel.
  • Gum probe: blunt, with a ball about 0.5 mm across and filed rings at 3.5 and 5.5 mm. Slide it gently between tooth and gum until it stops. Healthy: 1–3 mm. Over 4 mm is gum disease; over 6 mm, serious bone loss.

Scalers and excavators

  • Sickle scaler: a curved blade 10–12 mm long ending in a point, triangular in section, with two cutting edges, for tartar above the gum. A curette has a rounded toe and half-round back so it slides under the gum without cutting it.
  • Excavators: sharp-rimmed spoons 1, 1.5 and 2 mm across, two sizes on one handle, for scooping out soft decay.

Making them. Forge 5 mm bar to a tapered shank 2–3 mm thick, file the working end while soft, bend the shank, harden from cherry red, polish bright and temper straw (about 230 °C). Hollow excavator spoons with a small round burr.

Sharpening is the skill that matters. Rub each side of a scaler blade on a fine oiled stone, keeping the angle between face and side at 70–80°; finish on a hard fine stone or smooth slate. Test: drag the edge lightly across a thumbnail. Sharp bites and shaves a curl; blunt slides. Blunt scalers polish tartar smooth instead of lifting it. Sharpen after every two or three patients.

Filling instruments and mixing slab

  • Flat plastic ("shaping"): a thin blunt blade about 2 mm wide, for carrying and smoothing filling.
  • Plugger: a flat-ended rod 1–2 mm across, for packing filling into corners.
  • Mixing slab: thick glass 15 × 8 cm, at least 1.5 cm thick, with a flexible steel spatula. A thick, cool slab slows the cement's set.

These are tempered blue or left soft, and polished so filling does not stick.

Extraction instruments

Elevators

A narrow steel lever that loosens a tooth in its socket; it does most of the work of an extraction (Dentistry).

  • Straight elevator: blade 3–5 mm wide and 12–15 mm long, hollowed like a gouge, with a thin rounded end, on a 5–6 cm shank and a pear-shaped handle that fills the palm. Overall about 16 cm.
  • Root elevators: narrower, 2–3 mm, often in left and right pairs.

Forge from 8 mm steel and temper purple to blue (about 280–300 °C). It must never snap: a broken tip lost in a socket is a disaster. Test each new one by levering hard in a hardwood block; it may bend a little, never crack.

Danger A slipping elevator is the commonest serious injury in tooth-pulling. It can stab through the palate, the floor of the mouth or the cheek. Always rest a finger of the working hand on the jaw, keep the other hand's fingers either side of the tooth to feel and guard, and never lever against a healthy neighbour.

Extraction forceps

Pliers whose beaks slide down under the gum to grip the root, not the crown, which would break.

Upper straight forceps box joint — no side play beaks 15–20 mm handles 11–12 cm Lower universal forceps beaks at a right angle overall 16–18 cm tempered blue: tough Beaks on a root hollow beaks touch on two lines each Upper molar point fits between roots Good Bad tips meet, gap behind heels meet: slides off
Fig. 2 Extraction forceps. Upper forceps are nearly straight, lower forceps bent at a right angle. The beaks are hollow inside, so they grip the root at two lines. Upper molar forceps are made in left and right pairs because the cheek-side beak has a point that fits between the two outer roots.
Forceps Shape For
Upper straight Beaks in line with handles Upper front teeth and premolars
Upper molar, left and right Cheek-side beak with a central point Upper molars
Lower universal Beaks at a right angle Lower front teeth and premolars
Lower molar Right-angled, both beaks pointed ("cowhorn": long curved points that slide between the roots) Lower molars
Root forceps Fine narrow beaks Broken roots, children's teeth

Sizes. Overall 16–18 cm; handles 11–12 cm; beaks 15–20 mm long and 5–7 mm wide, hollowed inside to the curve of a root and finely cross-filed near the tip. Closed, the tips meet with a narrow gap behind, so they grip on two lines.

Making them is heavy scissor work (Scissors, Shears and Folding Knives, Blacksmithing). Forge two halves from 10–12 mm square high-carbon bar. The simplest joint is a lap joint with a 4–5 mm rivet; the better box joint, where one half passes through a slot in the other, cannot twist sideways and let the beaks slip. Bend the beaks hot over a 7 mm mandrel, temper the whole to blue (about 300 °C) for toughness, and polish every surface, especially inside the joint.

Good: tips meet; beaks stay parallel gripping a 6 mm rod; no side play; no sharp outer corners. Bad: heels meet first (they slide off), a loose joint, rough hollows.

The dental drill

A dental drill (dental engine) spins a small burr at 1,000–3,000 turns a minute while it is held like a pen. Before electric motors, it was driven by foot.

BURRS, MUCH ENLARGED Roundhead 0.8–2.5 mm Inverted coneflat floor, undercuts Fissurecuts the walls shank 2.35 mm Flywheel35–45 cm, heavy rim Endless cordsilk or gut, 3 mm Columnabout 1.2 m tall Jointed arma small pulley at each joint Handpiecesteel spindle,burr in a collet Treadle60–80 strokes a minute → 1,200–1,600 turns at the burr
Fig. 3 The treadle dental engine. The foot rocks the treadle, which turns a heavy flywheel. An endless cord runs from the big pulley up the column and over small pulleys at each joint of the arm to the handpiece, so the burr can be moved anywhere in the mouth while it keeps turning. The burr shapes are shown at the right, much enlarged.

Simplest: a burr in a handle twirled between finger and thumb, or a tiny bow drill. Both work for small holes; both are slow and hard to control.

The treadle engine is built like a small treadle lathe (The Lathe, Belts, Chains and Power Transmission):

  1. Base and treadle: a heavy base, and a foot treadle with a crank rod to a crank on the flywheel axle (Cranks, Cams and Linkages).
  2. Flywheel: 35–45 cm across, with a heavy rim (5–8 kg) and a V-groove. Its weight keeps the burr turning between strokes.
  3. Column: an iron tube about 1.2 m tall.
  4. Arm: two or three light jointed sections, 25–30 cm each, with a small grooved pulley (3–4 cm) at every joint so the cord runs at any angle.
  5. Cord: endless braided silk or gut, about 3 mm, joined with a tiny hook and eye and kept taut by a spring.
  6. Handpiece: a brass tube 12–14 cm long and 10–12 mm thick, a steel spindle in two bearings, a 2 cm pulley at the back and a split collet at the front to grip the burr.

A 40 cm flywheel driving a 2 cm pulley steps up 20 times: 60–80 treads a minute give 1,200–1,600 turns at the burr. Slow by modern standards, but it cuts enamel in minutes instead of an hour.

Good: no visible wobble at the burr tip; the cord stays on when the arm swings; the handpiece stays cool after five minutes. Bad: side play in the spindle (the burr chatters and cracks enamel), or a warm handpiece (oil it or ease the bearings). A right-angle head with tiny bevel gears (Gears) for back teeth is a later, watchmaker's job (Watches and Small Clocks).

Dental burrs

A burr (dentists write bur) is a small steel shaft with a cutting head. Make every shank exactly 2.35 mm across and about 44 mm long so all fit the same collet.

Shape Head Use
Round 0.8–2.5 mm Opening holes, removing decay, undercuts
Inverted cone 1–2 mm Flat floors, undercut walls
Fissure (cylinder) 1–1.5 mm × 4 mm Side walls, grooves
  1. Draw high-carbon wire to 2.35 mm (Iron and Brass Wire) and check each length in a gauge hole (Measurement from Scratch).
  2. Turn the head on a small lathe with a graver.
  3. Cut 6–8 flutes with a three-cornered needle file or graver, turning the burr evenly between cuts with a notched index disc on the spindle.
  4. Harden the head from cherry red in water or brine; temper pale straw (about 220 °C). Enamel is very hard.

A good burr cuts a smooth hole in a pulled tooth or bone without squealing. One that squeals and leaves black marks is blunt. Carbon steel dulls fast on enamel: keep plenty.

Warning Heat kills the pulp. Use light touches of a second or two, never steady pressure, and have a helper drip cool boiled water onto the burr from a squeeze bulb (Syringes and Hypodermic Needles).

Fillings

A tooth filling replaces tooth lost to decay. The plain zinc oxide–clove oil filling is in Dentistry; here is how to prepare the hole so a filling stays, and the stronger materials.

1 Decaysoft, dark, under a small hole 2 Cut outhard floor; walls undercut 3 LineZOE over the deepest point 4 Fill and carveshape it; check the bite undercut enameldentinepulpdecayliningcement or amalgam
Fig. 4 Preparing a cavity and placing a filling. The decay is cut out until the floor is hard; the side walls are cut slightly undercut so the filling locks in; a soothing lining goes over the deepest part; then cement or amalgam is pressed in and carved to the shape of the tooth.

Preparing the hole

  1. Isolate: boiled cotton rolls between cheek and tooth (and under the tongue for lower teeth). Most fillings fail if saliva wets them while setting.
  2. Open the enamel with a small round burr just wide enough to reach all the decay.
  3. Remove all soft decay with a larger round burr at slow speed or with excavators. Dark, hard dentine may stay; soft or leathery dentine must go.
  4. Shape with an inverted cone: a flat floor, walls very slightly undercut (wider at the bottom), and no thin unsupported enamel at the edge.
  5. Rinse and dry with boiled water and a twist of cotton.
  6. Line deep holes: if the floor is within about 1 mm of the pulp (pinkish through the dentine), put a thin layer of zinc oxide–clove oil over the deepest point only.

Zinc oxide–eugenol (ZOE)

Zinc oxide and clove oil, 4–6 parts powder to 1 of oil by weight, mixed to a stiff putty (Dentistry). About one-fifth powdered pine resin (rosin, Tar, Pitch and Glue) in the powder makes it set faster and harder. ZOE soothes and seals and lasts months to a year or two; it is the right choice for deep holes, milk teeth, and teeth awaiting a permanent filling, but too soft for heavy biting for long.

Zinc phosphate cement

Harder, and the standard dental cement for a century.

  • Powder: zinc oxide fired at bright red heat (about 1,000 °C) for an hour in a clay crucible (Firebrick and Refractories), with about one-tenth magnesia (Magnesium) if you have it, then ground very fine. Firing slows the set.
  • Liquid: phosphoric acid (Phosphoric Acid and Phosphates) diluted to 50–60 %, with about 5 % zinc oxide dissolved in it. Keep it tightly stoppered; it takes up water from the air.
  • Mix on a cool slab: draw the powder into a drop of liquid a little at a time over about 90 seconds, spreading widely to lose heat, until a lump lifted on the spatula pulls a thread of about 1 cm that snaps back.
  • Place with the flat plastic, pack with the plugger, smooth. Have the patient bite on thin paper rubbed with charcoal; scrape down any black mark. It sets in 5–8 minutes.

Warning Zinc phosphate is acid while it sets and will kill the pulp of a deep tooth. Always line deep holes with ZOE first, thin and only over the deepest point.

Amalgam, in outline

Amalgam is a powdered alloy (about 65–70 % silver, 25–29 % tin, a few % copper) mixed with nearly its own weight of mercury (Mercury). The mercury dissolves the particle surfaces into a paste that sets hard in minutes as new crystals grow, reaching full strength in a day. It is packed in small amounts with a plugger and carved. It is strong, cheap and long-lasting, but mercury vapour slowly poisons whoever mixes it day after day. Do not make amalgam without ventilation, sealed mixing, a trap for every scrap, and training.

Glass ionomer, in outline

A fine powder of glass melted from silica, alumina and calcium fluoride, mixed with a water solution of polyacrylic acid. The acid dissolves the glass surface and the released calcium and aluminium link the acid's chains into a hard gel. It sticks chemically to tooth (no undercut needed) and slowly releases fluoride, protecting the tooth around it. The glass is within reach of a good Glass furnace, but polyacrylic acid needs petroleum chemistry (Petrochemicals and Modern Plastics): a goal for a later laboratory.

Sterilising instruments

Mouths carry hepatitis B and C and HIV. Every instrument must be sterile for the next patient (Sterilising Instruments and Dressings).

  1. Soak at once in cold soapy water so blood does not dry on.
  2. Scrub under water with a stiff brush, joints open, in thick gloves. Mind forceps joints, burr flutes and beak serrations.
  3. Inspect with a lens (Lenses): no dried matter, rust, blunt or bent tips.
  4. Sterilise: autoclave at 121 °C for 30 minutes or 134 °C for 15 minutes in cloth packs (20 and 4 minutes if unwrapped), as in Sterilising Instruments and Dressings. Dry heat, 160 °C for 2 hours, for burrs and carbon-steel cutters, which steam rusts. Boiling for 20 minutes only when nothing else exists, with a spoonful of washing soda per litre against rust (Soda Ash and Baking Soda).
  5. Store dry in closed, labelled packs. Oil the handpiece bearings after sterilising.

How to tell it worked

  • Instruments: the probe catches a fingernail lightly; the scaler shaves it; the elevator survives the wood block; forceps grip a 6 mm peg at the tips; burrs cut bone cleanly.
  • Fillings: no black mark on the filling when the patient bites on charcoal paper; cold no longer hurts after a day or two; a probe drawn across the edge does not catch. After a month it is still there, with no dark line round it.

Note Troubleshooting. Filling falls out → decay left, a wet hole, or walls flared outward. Clean, dry, undercut, refill. Tooth aches day and night after filling → the pulp is dying: too deep, overheated, or acid cement without a lining. Replace with ZOE; if pain continues, extract (Dentistry). Cement sets on the slab → slab too warm or powder added too fast. Forceps crush the crown → beaks not pushed far enough under the gum, or meeting at the heels. Burr wobbles → bent burr (it rocks when rolled on glass) or a worn bearing.

Dangers

Danger Inhaled and swallowed objects. A burr, a broken tip or a tooth can fall into the throat and be breathed into the lungs. Keep a gauze screen across the back of the mouth, never work with the patient lying flat, and count every small part after the job.

  • Cross-infection: shared unsterilised instruments have spread hepatitis through whole villages. One set, one patient, then sterilise.
  • Mercury poisons the dentist slowly: tremor, sore gums, mood changes.
  • Phosphoric acid burns eyes and lips; keep it in a stoppered dropper bottle and never pass it over the patient's face.
  • Hot instruments straight from the sterilizer burn the cheek; let them cool.
  • Know your limits: root canals, wisdom teeth and large broken roots need training beyond this book.

What this unlocks

With a drill and cement, most decayed teeth can be kept, so people chew well into old age (Nutrition and Deficiency Diseases). The small precision work — spindles, collets, burrs, indexing — feeds Watches and Small Clocks and Scientific Instrument Making, and the jointed cord arm was copied for engravers and jewellers (Engraving, Seals and Etching, Jewellery, Beads and Medals). Electric motors (The Electric Motor) and later air turbines (Bellows to Air Compressors) replace the treadle.

How it was first done

People at Mehrgarh, in today's Pakistan, drilled molars with flint-tipped bow drills about 9,000 years ago. Medieval surgeons pulled teeth with the "pelican", a lever-hook that often broke the jaw, and later with the "key". Pierre Fauchard (1728) described hand drills and fillings of lead and tin. The English dentist John Tomes designed forceps shaped to each kind of tooth in the 1840s. James Beall Morrison of the United States patented the foot-treadle dental engine in 1871; electric engines followed within years, and air-turbine drills in the 1950s. Zinc oxide–eugenol came into use in the 1870s and zinc phosphate cement around 1880. G. V. Black of Chicago set the rules for shaping cavities and standardised amalgam alloy in the 1890s. Glass ionomer was invented by Alan Wilson and Brian Kent in Britain around 1969–1972.

Source: content/entries/health/dental-instruments.md