Two rare elements that hide in sulfide ores and turn up in the red mud of sulfuric acid works and the black slime of copper refineries. How to find and recover them, purify selenium and turn it into the grey, light-sensitive form that made the first photocells, light meters and dry rectifiers — and how to avoid being poisoned by them.
- Difficulty
- ●●●●●
- Time
- Months to collect enough sludge or slime; a few days for one recovery; a day to make and anneal a cell
- Steps from zero
- 14 prerequisites →
This unlocks
Photocells and SensorsThe full path from nothing — 14 steps before this one
- Fire
- Finding and Preparing Clay
- Sulfur
- Pottery
- The Kiln
- Lime
- Lye and Potash
- Fermentation
- Glass
- Acids, Bases and Testing
- Saltpeter
- Laboratory Glassware
- Sulfuric Acid
- Identifying Substances
- Selenium and Tellurium
Do them roughly in this order. See it on the tech tree →
Why it matters
Selenium is the element that first showed that light can change electricity. In the 1870s a bar of grey selenium was found to conduct better in light than in the dark. That discovery gave the photophone, the first television experiments, the photographer's light meter, the electric eye that counts things on a belt and opens doors, and later the photocopier. Grey selenium also conducts one way better than the other, and for thirty years selenium rectifiers turned the AC mains into DC in every radio and battery charger (Rectifiers: Turning AC into DC).
Selenium also matters in the glassworks — a trace of it cancels the green tint that iron gives to cheap glass, and with cadmium it makes the deep red of signal lamps — and on the farm: animals and people need a tiny amount and are poisoned by a little more.
Tellurium, its heavier cousin, makes copper and lead tougher and easier to machine, and as bismuth telluride is the best material for the thermoelectric coolers and generators of Thermocouples and Thermoelectricity.
Be honest about scale. Selenium is rare: refining a tonne of copper gives only around 100–200 g of it. Gathering enough for a few cells and rectifier plates takes a working Sulfuric Acid plant or copper refinery (Electrolysis) and patience. But a few hundred grams is enough to do a great deal.
How it works
Selenium and tellurium sit directly below sulfur in the family of elements (Atoms, Elements and Reactions). They behave like sulfur: they burn to an oxide, form "-ide" compounds with metals, and travel with sulfur in nature. That is why they are found in sulfide ores — pyrite, copper pyrites, lead and gold ores — and why, when those ores are burned or refined, they follow the sulfur and then drop out where it does not.
Selenium comes in three main forms:
| Form | Looks like | How you get it |
|---|---|---|
| Red (amorphous) | Brick-red powder | Thrown out of solution by sulfur dioxide, cold |
| Black glassy | Shiny black, brittle like pitch, red when thin | Melted selenium cooled quickly |
| Grey (crystalline, "metallic") | Dull grey, metal-like | Red or black selenium held near 200 °C for hours |
Only the grey form is useful in electrical work. It is a semiconductor (Semiconductors and the Transistor): in the dark it barely conducts, but light frees electrons in it, and its resistance falls several times over in bright light. Where grey selenium meets certain metals, it forms a one-way junction — the basis of the selenium cell that makes its own current (Solar Cells) and of the rectifier.
Selenium melts at 221 °C and boils at 685 °C. Its oxide, selenium dioxide, turns straight from solid to vapour at about 315 °C and dissolves easily in water as selenous acid. That pair of facts gives the simplest recovery: oxidise, sublime the oxide away from everything else, dissolve it, and pull the oxygen out again with sulfur dioxide. Tellurium's oxide does not sublime at that heat, so it stays behind.
What you need
| Item | Use | Notes |
|---|---|---|
| Sludge or slime: red-brown lead-chamber mud, flue dust from pyrite burners, or anode slime | Raw material | Sulfuric Acid, Electrolysis |
| Strong nitric acid | Oxidising selenium | Nitric Acid |
| Porcelain dishes, a hard-glass or fireclay tube 60–80 cm long, flasks | Evaporating, subliming | Stoneware and Porcelain, Laboratory Glassware |
| Sulfur and a gas bottle | Making sulfur dioxide | Sulfur |
| Hydrochloric acid, lye | Separating tellurium | Hydrochloric Acid, Lye and Potash |
| Burner, sand bath, filter paper, funnel | Heating and filtering | Burners, Stands and Laboratory Equipment |
| A place outdoors with a strong wind, or a fume chimney | Safety | See Dangers |
Where to find it
- Lead-chamber and flue mud. Where pyrite or copper pyrites is roasted for Sulfuric Acid, selenium leaves with the gas and settles as a red to red-brown mud in the bottom of the chambers, the dust chambers and the first wash towers. Acid made from volcanic sulfur may carry it too. Selenium was discovered in exactly this mud.
- Anode slime. When impure copper is refined by Electrolysis, selenium, tellurium, silver and gold fall from the anodes as a black slime in the bottom of the tank. Slime commonly holds 5–20 % selenium and a few percent tellurium — the richest source. Recover the silver and gold afterwards from what is left (Gold and Silver).
- Ores. Pyrite and chalcopyrite (Finding and Identifying Ores) hold traces; some copper and lead ores, and the sulfur of some volcanoes, hold more. Pure selenium minerals are rare curiosities.
- Tellurium is richest in the gold tellurides — heavy, brittle, silver-white to brassy crystals in gold veins (Transylvania, Colorado, Western Australia) — and in copper anode slime.
- Seleniferous land. On some dry plains, certain plants — milkvetches (Astragalus), prince's plume, woody aster — collect so much selenium from the soil that they smell of garlic and poison livestock. These mark selenium-rich soil, not a practical source.
Tests (Identifying Substances):
- Smell. Heated on charcoal before the blowpipe, selenium compounds give a reek of rotting horseradish and a brown-red fume; this smell alone is a strong sign. (Do it once, briefly, outdoors.)
- Colour in strong sulfuric acid. Warm a crumb of the dried mud with strong sulfuric acid: selenium dissolves to a green liquid; tellurium gives a carmine red one. Pour the acid into water: selenium falls out as a red powder, tellurium as a black one.
- Red precipitate. Dissolve some mud in nitric acid, dilute, add a little hydrochloric acid and bubble in sulfur dioxide: a brick-red cloud means selenium.
Method 1: Recovering selenium in the laboratory
This route works for a few hundred grams of mud or slime at a time.
- Wash and dry. Stir the mud or slime with plenty of water, let it settle, and pour off the acid water; repeat until the water is no longer sour. Dry it.
- Dissolve in nitric acid. Outdoors, in a porcelain dish or a large flask on a sand bath, warm 1 part mud with 3–4 parts strong nitric acid by weight, adding the acid in portions. Choking brown fumes come off; let them blow away. Selenium becomes selenous acid in solution. Lead stays behind as white sulfate, and much of the copper and silver dissolve. Dilute with a little water and filter.
- Boil to dryness. Evaporate the filtrate in a porcelain dish until a dry crust remains, then heat it more strongly to drive off all nitric acid. The crust holds the selenium as selenium dioxide.
- Sublime. Put the crust in a hard-glass or fireclay tube, closed at one end or plugged loosely with glass wool, lying nearly flat. Heat the end holding the crust to about 350–400 °C — dull red just showing in the dark — while drawing a very slow stream of air through the tube with a water-jet or bellows. White needles of selenium dioxide grow in the cooler part of the tube. Tellurium, copper, silver and other metals stay behind in the residue. Scrape out the needles when cool.
- Dissolve and reduce. Dissolve the needles in about ten times their weight of water with a little hydrochloric acid. Bubble sulfur dioxide through it — made by burning sulfur in a closed jar with a draught of air, or by heating copper with strong sulfuric acid in a flask (Sulfur). A brick-red powder of selenium falls at once. Keep bubbling until a fresh drop of the liquid gives no more red.
- Make it grey. Heat the liquid with the red powder to boiling. In a few minutes the red turns dark grey to black and clots into a dense powder that filters easily. Filter, wash with water until the washings are not acid, and dry.
- Melt. Melt the grey powder in a covered porcelain crucible at about 250 °C — just enough to melt tin — and pour it onto a cold glazed tile or into a groove in a slab to make black sticks. These are handy for coating cell and rectifier plates.
For greater purity, distil the selenium in a hard-glass retort (it boils at 685 °C, bright red heat), or repeat steps 2–6. One pass gives selenium good enough for cells; rectifier and photocopier selenium was made 99.99 % pure.
Recovering tellurium
Grind the residue left in the tube and boil it with lye (caustic soda solution, Lye and Potash): tellurium dissolves as sodium tellurite. Filter, and slowly add dilute sulfuric acid until litmus turns just faintly red: white tellurium dioxide settles out. Dissolve that in hydrochloric acid and bubble sulfur dioxide through it: black tellurium powder falls. Wash, dry and melt it under a layer of borax at about 450–500 °C (Borax and Boric Acid). It is a brittle, silvery-white metal-like solid.
Method 2: Recovery at the works
At a sulfuric acid plant or copper refinery, slime is handled by the bucketful:
- Sulfating roast. Mix the slime with strong sulfuric acid to a paste and roast it in an iron pan or a slowly turning kiln at 300–600 °C. Selenium dioxide and sulfur dioxide leave together. Led through towers sprayed with water, they react: the sulfur dioxide pulls the oxygen from the selenous acid, and red selenium settles as mud in the tank under the towers. The roast residue goes on to tellurium, silver and gold recovery.
- Soda roast. Roast the slime with soda ash; selenium becomes a salt that dissolves in water. Leach, neutralise to drop out tellurium oxide, then bubble in sulfur dioxide for the selenium.
Either way, the furnace gases must go up a tall stack after scrubbing, never into a workroom.
Making grey selenium devices
The selenium cell (light-sensitive resistor)
This is the oldest and easiest electric eye: a film of grey selenium between two interleaved combs of wire. Its resistance is high in the dark and falls several times over in bright light.
- Former. A flat plate of slate, mica or glazed tile about 3 × 5 cm.
- Wires. Wind two separate bare copper or brass wires (0.3–0.5 mm) side by side round the plate, keeping a gap of 0.5–1 mm between neighbouring turns — like a two-start screw thread. The wires must never touch. One wire ends at one terminal, the other at the second terminal.
- Coat. Warm the plate to about 230 °C on a hotplate or sand bath and rub a stick of selenium over one face so it melts into a thin film filling the gaps between the wires.
- Anneal. Hold the plate at 190–210 °C — just below melting — for several hours, until the shiny black film turns dull grey. This step makes the cell. Cool slowly.
- Protect it under glass sealed with wax, or in a small box with a window.
- Test. Connect it in a circuit with a battery and a galvanometer (Measuring Electricity). Shade it with your hand, then uncover it in daylight: the current should rise three to twenty times. It responds within a fraction of a second, but its recovery in the dark is slow.
A cell like this, with a battery and a sensitive relay, rings a bell when a beam is broken, lights street lamps at dusk, and counts objects passing a lamp (Photocells and Sensors). The self-generating selenium cell, which needs no battery and makes a light meter, is described in Solar Cells.
The selenium rectifier plate
The construction of rectifier stacks and how to use them is in Rectifiers: Turning AC into DC. Making the plates:
- Base: a flat plate of aluminium or nickel-plated iron, 2–5 cm across, roughened with fine sand.
- Coat it with a film of selenium about 0.05–0.1 mm thick, melted on and pressed flat with a warm, smooth plate. A trace of iodine or bromine in the selenium (about one part in ten thousand) makes better plates.
- Anneal at 200–215 °C for about an hour to turn it grey and crystalline.
- Top contact: a thin layer of a low-melting alloy of tin and bismuth, sprayed or pressed on while warm, leaving a bare margin round the edge.
- Form the plate: pass a small reverse current (from the alloy side to the base) at a voltage raised slowly over several hours to the working value. This builds the thin barrier layer at the alloy contact that gives the one-way action.
A good plate passes current easily from the base into the selenium with a drop of about 1 V, and blocks it the other way up to about 20 V. It carries roughly 50 mA per square centimetre; stack plates in series for higher voltages.
Other uses
- Glass. A trace of selenium added to the batch turns glass faintly pink, which cancels the faint green of iron, giving "white" glass from ordinary sand. The dose is tiny — roughly a few grams to a few tens of grams per tonne of sand, and most of it burns off in the furnace — so start with about 0.1 g per 10 kg of batch and find the right amount by trial melts; too much turns the glass pink or brown (Glass). With cadmium sulfide, selenium gives the clear, deep selenium ruby of railway and traffic lamps (Railway Signalling and Safety) and the bright cadmium red pigment (Pigments, Paints and Varnish); cadmium is poisonous in its own right.
- Metals. A few tenths of a percent of selenium or tellurium in copper or steel makes it cut cleanly on a lathe; a little tellurium hardens lead for cable sheaths and battery parts (Lead).
- Rubber. Selenium and tellurium speed vulcanisation of some rubbers (Rubber).
- Thermoelectric couples. Bismuth telluride, melted from bismuth (Antimony and Bismuth) and tellurium, makes small coolers and generators that work at room temperature (Thermocouples and Thermoelectricity).
- Photocopying. A drum coated with glassy selenium holds an electric charge in the dark and loses it where light falls — the heart of the first office copiers (Copying Documents and Xerography).
Selenium in food and farming
Animals and people need selenium in micrograms: an adult needs about 55 µg a day, and more than about 400 µg a day for months begins to poison. Too little causes white muscle disease in lambs and calves on poor soils (stiff, weak, dying young), and in parts of China a heart disease of children (Keshan disease). Too much — livestock grazing selenium-collecting plants on seleniferous plains — causes "alkali disease": hair loss, cracked and falling hooves, lameness and blindness. Where white muscle disease is common, give stock only measured, ready-mixed supplements or salt licks under advice from someone who knows the local soil (Animal Health). Never dose animals or people with home-made selenium salts: the gap between enough and too much is small.
How to tell it worked
- Red selenium comes down at once when sulfur dioxide reaches the liquid; grey selenium is a dull grey, brittle solid that melts at the heat that melts tin (221 °C against tin's 232 °C) to a black liquid.
- A crumb warmed in strong sulfuric acid colours it green.
- A good cell changes its current several times over between hand-shadow and daylight; a good rectifier plate passes current easily one way and very little the other (Measuring Electricity).
Note Troubleshooting.
- No needles in the tube → too little heat, or the crust still wet with nitric acid; dry it fully, then heat to dull red.
- Red selenium will not turn grey → boil longer; it changes faster above 90 °C.
- Selenium film stays shiny black → annealing too cool or too short; keep it at 200 °C for longer, never above 221 °C or it melts and must start again.
- Cell shorted → the two wires touch somewhere; rewind with a wider gap.
- Cell barely responds → film too thick, or not fully grey.
- Rectifier leaks backwards → not formed long enough, or alloy touching the base at the edge.
Dangers
Danger Selenium and tellurium compounds are poisons. Selenium dioxide burns skin and eyes and is poisonous breathed as dust or fume; hydrogen selenide — formed when acids touch selenides — is more poisonous than hydrogen sulfide (a few breaths of a strong concentration can kill) and soon numbs the nose. Do every heating, subliming and sulfur-dioxide step outdoors or under a strong chimney draught, upwind, wearing gloves and goggles. Never heat selenium above about 250 °C in the open, except in a closed retort.
- Warning signs. A garlic smell on the breath without eating garlic, a metallic taste, red, sore eyes, tiredness, and later loss of hair and nails mean you are absorbing selenium or tellurium. Stop work, wash, and do not return until the smell has gone. Tellurium gives a garlic breath that can last for weeks from a tiny dose.
- Nitric acid fumes and sulfur dioxide in these methods damage the lungs (Nitric Acid, Sulfur).
- Waste. Selenium-bearing liquids kill fish and birds in ponds and marshes. Bubble sulfur dioxide through all wash waters to drop out the last red selenium, collect it, and bury what cannot be used in a lined, dry pit far from water.
- Overheated selenium rectifiers smell foul and give off poisonous fumes: switch off and ventilate.
- Cadmium used for selenium ruby glass and pigments is a poison in its own right.
What this unlocks
Selenium cells give the first electric eyes and light meters (Photocells and Sensors, Photography), the photocells of early Cathode Rays and Television and sound-on-film, and the dry rectifiers that power Radio sets and battery chargers from the mains (Rectifiers: Turning AC into DC). Working with selenium teaches the habits of Semiconductors and the Transistor: purity, careful heat treatment and junctions. Tellurium leads to thermoelectric coolers and, much later, to cadmium-telluride Solar Cells.
How it was first done
Tellurium was found first, by the Austrian mining official Franz-Joseph Müller von Reichenstein in 1782, in gold ores from Transylvania; Martin Heinrich Klaproth named it in 1798 after tellus, the earth. In 1817 the Swedish chemists Jöns Jacob Berzelius and Johan Gottlieb Gahn, partners in a sulfuric acid works at Gripsholm that burned pyrite from the Falun copper mine, investigated a red mud in their lead chamber. They first took it for tellurium because of its smell, then found a new element and named it selenium, after selēnē, the moon — tellurium's companion. In 1873 the English telegraph engineer Willoughby Smith, testing selenium bars as high resistances for submarine cables, found that their resistance changed with light. Alexander Graham Bell used selenium in his light-beam "photophone" of 1880, and Charles Fritts made the first selenium solar cells in New York in 1883. Selenium rectifiers came into wide use in the 1930s, and the first automatic office copier, the Xerox 914 of 1959, used a selenium drum.