◆ Rebuild

Part 13 · Electricity

Transformer Steel, Ferrite and Magnetic Shielding

The iron inside every transformer, motor, choke and radio coil, and the metal boxes that keep stray magnetism out. Soft iron for steady fields; silicon steel rolled thin and insulated for mains power; pressed iron powder and fired ferrite ceramics for radio and switch-mode supplies; nickel–iron alloys for sensitive transformers and magnetic shields — how each is made, cut and judged.

Difficulty
●●●●●
Time
A week to anneal and insulate a stack of hand-cut laminations; a season to set up rolling and punching; a month of trials for a first good ferrite
Steps from zero
32 prerequisites →

You need first

The TransformerAlloy and Stainless Steels

This unlocks

—
The full path from nothing — 32 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Bricks
  13. Fermentation
  14. The Wheel and Axle
  15. Firebrick and Refractories
  16. Bellows
  17. Gears
  18. Copper Smelting
  19. Iron (the Bloomery)
  20. The Waterwheel
  21. Blacksmithing
  22. The Blast Furnace and Cast Iron
  23. The Battery
  24. Magnets
  25. Steel
  26. Copper Wire
  27. Steel in Quantity
  28. The Electromagnet
  29. The Generator
  30. The Electric Arc Furnace
  31. The Transformer
  32. Alloy and Stainless Steels
  33. Transformer Steel, Ferrite and Magnetic Shielding

Do them roughly in this order. See it on the tech tree →

Why it matters

A The Transformer wound on varnished iron wire works. But a whole country's transformers and motors can waste a large share of its electricity heating their cores, and the right iron cuts that loss to a few per cent. Silicon steel, rolled thin and stamped into laminations, made the Power Lines and Distribution economic.

At higher frequencies even the best sheet steel fails. A radio coil at a million cycles a second, or a switch-mode supply at 50,000, needs a core that is magnetic but does not conduct: pressed iron powder or a black fired ceramic called ferrite. Other jobs need a shield that steers stray magnetism away from a cathode-ray tube, a sensitive meter or a compass.

These are the soft magnetic materials, which magnetise and let go easily. Materials that stay magnetised belong to Permanent Magnets.

How it works

Permeability and saturation

Iron is made of tiny regions, domains, each a small magnet pointing its own way. A coil's field swings them into line, multiplying its magnetism hundreds or thousands of times — the permeability. When all are lined up the iron is saturated and more current adds almost nothing: iron at about 2.1 tesla, ferrite at only about 0.4.

Where the power goes

  • Hysteresis loss. The domains stick a little each time they swing, like a stiff hinge. The loss grows with the number of swings per second. Impurities (carbon, nitrogen, sulfur) and strain from bending or punching make it worse; annealing relieves strain and grows large grains.
  • Eddy-current loss. Changing magnetism drives currents round inside the iron (The Transformer). This loss grows with the square of the frequency and the square of the sheet thickness, and falls as the metal's resistance rises. Halve the thickness and you quarter it.

Silicon, 3–4 %, raises iron's electrical resistance about fourfold, lowers hysteresis loss and stops plain iron's slow worsening ("ageing") in warm service. The price: slightly lower saturation and a brittle steel that must be rolled hot.

The right core for each job

Material Permeability Saturates at Use
Annealed soft iron 1,000–5,000 2.1 T Steady fields: relays, electromagnets, poles
Silicon steel, 0.35–0.5 mm 1,000–8,000 2.0 T 50–60 Hz transformers, motors, chokes
Grain-oriented silicon steel to 30,000 along the roll 2.0 T Large power transformers
50 % nickel–iron 5,000–40,000 1.5 T Audio and small precise transformers
78 % nickel–iron (permalloy, mu-metal) 20,000–100,000 0.7–0.8 T Shields, signal transformers
Pressed iron powder 4–100 1.0–1.5 T Chokes 10–500 kHz; radio coils to 200 MHz
Manganese–zinc ferrite 1,000–15,000 0.4–0.5 T Switch-mode transformers, 10 kHz–1 MHz
Nickel–zinc ferrite 10–1,500 0.3–0.4 T Radio 1–500 MHz, aerial rods, beads

What you need

Item Details
Low-carbon steel or wrought iron Under 0.05 % carbon (Steel in Quantity, Iron (the Bloomery))
Ferrosilicon About 75 % silicon, from quartz, iron and coke in the The Electric Arc Furnace (Alloy and Stainless Steels)
Nickel Electrolytic (Nickel and Cobalt)
Rolling and punching A hot mill (Sheet Metal and Rolling); a fly or power press with hardened E-and-I dies (Presses, Punches and Dies)
Annealing furnace 800–1,150 °C, closed steel boxes, dry hydrogen or cracked ammonia (Electric Kilns and Furnaces, Ammonia, Hydrogen, Oxygen and Gases)
For ferrite and powder Pure oxides; a porcelain ball mill (Stoneware and Porcelain); a kiln to 1,350 °C (The Kiln); a hydraulic press (Hydraulic Presses and Rams)
Insulation Shellac or varnish (Pigments, Paints and Varnish), tissue Paper, phosphoric acid (Phosphorus)
Testing Compass, magnet, meter, signal generator or inductance bridge (Electronic Test Equipment)

Where to find it

Iron as in Iron (the Bloomery) and Finding and Identifying Ores — phosphorus and sulfur spoil magnetic quality. Quartz for ferrosilicon (Pure Silicon). Nickel from green garnierite and sulfide ores (Nickel and Cobalt). Manganese from black, finger-staining pyrolusite (Alloy and Stainless Steels). Zinc oxide by burning zinc (Zinc and Brass). Pure red iron oxide: dissolve clean iron scrap in dilute Sulfuric Acid, recrystallise the green vitriol two or three times, and roast it at 700–800 °C to a soft purple-red powder. Natural magnetite and hematite are too impure for ferrite — though a lodestone (Magnets) is itself a natural ferrite.

Soft iron

For steady magnetism — relay and electromagnet cores (The Electromagnet), the poles of a The Generator or The Electric Motor, The Telegraph armatures — use the purest soft iron, finished and then annealed: pack it in a closed steel box with clean sand or iron scale (not charcoal, which adds carbon), hold at 850–900 °C (bright cherry red) an hour per 25 mm of thickness, and cool in the furnace overnight. Do not hammer or bend it afterwards. A good relay core drops its armature the instant the current stops; if it hangs on, anneal again or fit a thin brass shim on the pole face.

Silicon steel laminations

Making and rolling the steel

  1. Refine low-carbon steel in an open-hearth or electric furnace to below 0.03 % carbon, and add ferrosilicon in the ladle for 3–3.5 % silicon (motors) or 4–4.5 % (transformers). More is too brittle to roll.
  2. Pack-roll: heat a pack of 3–8 sheet bars to bright red (800–900 °C) and roll them together; double the pack, reheat, roll again, down to 0.35–0.5 mm. Rolling several at once stops thin sheets cooling too fast.
  3. Box-anneal: stack the sheets in a sealed steel box, hold at 800–900 °C for a day, and cool over another. A little damp air in the box burns out the last carbon.
  4. Pickle off the scale in warm dilute sulfuric acid.

This hot-rolled route made nearly all transformer steel from about 1905 into the 1950s. Grain-oriented steel (Norman Goss, 1934) is cold-rolled in two stages with a decarburising anneal between, then annealed at 1,150–1,200 °C in dry hydrogen for a day or two. Its grains grow centimetres across, all with their easy direction along the roll, and its loss falls to under 1 watt per kilogram at 1.5 T and 50 Hz — a third or less of hot-rolled steel. It needs a powerful cold mill and hydrogen furnaces.

Insulating the sheets

  • Oxide: open the annealing box at about 500 °C to air or steam; the sheets turn blue-black. Enough for small cores.
  • Paper: tissue 0.03 mm thick glued to one side — the old way, but it wastes space.
  • Varnish: one thin baked coat of shellac or varnish, 5–10 µm.
  • Phosphate: dip in hot dilute phosphoric acid with a little magnesium or aluminium dissolved in it, and bake at 400–500 °C. A hard grey film that survives later annealing: the modern standard.

Bulb test: clamp one coated sheet between two flat brass plates wired through a torch battery and bulb. The bulb must not light.

Punching E and I laminations

aa2aaaa3aa Punching two E's face to face; the slots are the two I's One layer I across the tips of the E coil sits on the 2a tongue (copper, in the two windows) Alternate layers odd even joints overlap for a choke: all E's one way, paper gap at the joint
Fig. 1 The scrapless E–I lamination. Two E's punched face to face leave two slots between them, exactly the size of the two I pieces, so one rectangle of sheet gives a full layer with no waste. In the core, the E's and I's are laid the other way round on alternate layers so the joints overlap like brickwork.

The scrapless E–I pattern, in a size unit a: centre tongue 2a wide (the coil sits on it); outer legs and yoke a; each window a × 3a; E 6a × 4a; I 6a × a; assembled core 6a × 5a. For a 100 W, 50 Hz transformer needing about 10 cm² of iron (The Transformer), a = 1.6 cm gives a 3.2 cm tongue; stack it 3.3 cm thick.

  1. Dies of hardened tool steel, with clearance only 5–8 % of the sheet thickness (Presses, Punches and Dies).
  2. Punch E's in facing pairs; the slots between them are the I's.
  3. Feel for burrs. A burr you can feel (over about 0.02 mm) cuts the next sheet's insulation and the core runs hot. Regrind the dies.
  4. Anneal after punching, 750–800 °C for an hour in a closed box, cooling slowly: punching damages a strip one thickness wide along every cut. Do it before varnish or paper; oxide and phosphate survive it.

Building the core

  • Interleave for transformers: alternate the E's and I's layer by layer so each joint is bridged.
  • Butt-stack for chokes carrying direct current (Resistors, Capacitors and Coils): all E's together, all I's together, with a paper or card gap of 0.1–1 mm so the steady current does not saturate the iron.
  • Clamp hard between steel angles, with bolts in insulating paper tubes so they do not form a shorted turn. Loose cores hum.

Turns per volt (the The Transformer formula with better iron): plain iron 2,800 ÷ (Hz × cm²); hot-rolled silicon steel 1,900 ÷ (Hz × cm²); grain-oriented 1,450 ÷ (Hz × cm²). Better steel saves a third to a half of the copper.

Wound and cut cores

Grain-oriented steel works best when the magnetism always runs along the roll. Wind coated strip 0.1–0.3 mm thick tightly round a rectangular former, anneal it there at 800 °C, soak in varnish and bake solid. Saw it into two C halves with a thin abrasive wheel, lap the cut faces flat (Abrasives and Grinding Stones), slide them into the coil and pull them together with a steel band. A toroid is the same strip wound into an uncut ring: no waste, least hum, but the wire must be threaded through by hand or shuttle.

Powder-iron cores

Grind iron fine, coat each grain with insulation and press it solid: the core carries magnetism but not eddy currents. The insulation between grains acts as a distributed air gap, so the core tolerates direct current without saturating.

Powder: precipitate iron hydroxide from purified green vitriol with soda (Soda Ash and Baking Soda), dry, calcine to fine red oxide, and reduce in thin trays under dry hydrogen at 450–600 °C for several hours to grey-black iron of a few micrometres. (Industrial carbonyl iron, perfect spheres of 2–8 micrometres, is made through iron carbonyl, a highly poisonous gas.) Sieve finer than 50 micrometres for chokes, 10 for radio coils.

Pressing:

  1. Stir the powder with dilute phosphoric acid (0.5–1 % of the iron's weight) and dry: each grain gets a phosphate skin.
  2. Mix in 2–4 % shellac dissolved in alcohol, dry, and rub through a sieve into granules.
  3. Press in a hardened die at 5–10 tonnes per square centimetre for chokes (Hydraulic Presses and Rams); radio slugs may simply be moulded with more varnish.
  4. Bake at about 150 °C.

Shapes: rings for switch-mode chokes (Power Supplies and Regulators); threaded slugs screwed in and out of a coil former to tune a Radio coil (Resistors, Capacitors and Coils).

Ferrite cores

1 Weighpure oxides 2 Ball-millwet, 12–24 h 3 Calcine900–1,000 °C 4 Mill and press1–2 t per cm² 5 Sintershrinks about 1/6 6 Lap faceson glass with grit ironMn/Nizinc E coresswitch-mode transformers Pot coreshields its own coil Toroidchokes, wideband Rodmedium-wave aerial Beadstops interference Finished shapes
Fig. 2 Making a ferrite core. Weigh the pure oxides, mill them together in water, calcine, mill fine with a binder, press, and sinter — the part shrinks by about a sixth — then lap the mating faces flat. Below, the common shapes.

Ferrite is a ceramic of iron oxide with zinc and manganese or nickel oxides, made like porcelain. It comes out of the kiln black, hard and magnetic, with thousands to millions of times the electrical resistance of iron.

Ferrite (parts by weight) Red iron oxide Second oxide Zinc oxide Fire
Nickel–zinc (make first) 67 nickel oxide 16 17 1,150–1,250 °C in air
Manganese–zinc 70 manganese dioxide 23 11 1,250–1,350 °C, cooled without air

Purity matters more than in pottery: a few tenths of a per cent of silica or lime spoil it. Make the oxides as under Where to find it; nickel oxide by dissolving nickel in Nitric Acid, evaporating and heating the salt to green-black oxide.

  1. Mill the weighed oxides wet in a porcelain jar half-full of porcelain balls for 12–24 hours. Dry.
  2. Calcine at 900–1,000 °C for two hours. A magnet should now pick up the crumbs.
  3. Mill again for a day until flour-fine. Mix in 1–2 % dextrin, gum or wax as binder; dry and rub through a fine sieve.
  4. Press at 1–2 tonnes per square centimetre, in a die about 20 % larger than the finished part — it shrinks by 15–20 % in firing.
  5. Sinter: heat at about 2 °C a minute to 500 °C to burn out the binder, then to the firing heat; hold 2–4 hours and cool slowly. Nickel–zinc fires in ordinary air. Manganese–zinc must cool with almost no oxygen: pack the parts in a closed saggar in crushed old ferrite, or pass nitrogen through an electric kiln (Liquid Air, Nitrogen and the Noble Gases). Cooled in air, it gets a reddish skin and poor permeability.
  6. Lap mating faces on glass with fine abrasive until a pair meets with no line of light. For a gapped core, grind the centre leg shorter.

Shapes and uses

  • E and pot cores (a cup with a centre post, which also shields its coil) for switch-mode transformers. For a square wave at about 0.2 T, turns per volt ≈ 12,500 ÷ (Hz × cm²): at 50 kHz on a 1 cm² centre leg, a quarter turn per volt — three turns for 12 V.
  • Toroids for chokes and wideband transformers.
  • Ferrite rod antenna: a rod 8–10 mm across, 10–20 cm long, with about 60 turns of fine stranded wire tuned by a 365 pF variable capacitor. It gathers medium-wave signals as well as a long outdoor aerial, and turning it nulls an interfering station (Radio).
  • Beads slipped over a wire block radio interference.

Nickel–iron alloys

Iron with 36–80 % nickel has enormous permeability, if clean and properly annealed.

  1. Melt electrolytic nickel and pure iron in a magnesia or clay-graphite crucible (Electric Kilns and Furnaces). Mu-metal: 77 % nickel, 5 % copper, 2 % chromium or molybdenum, rest iron. Permalloy: 78 % nickel, 22 % iron. The tougher, cheaper 50 % alloy: equal parts. Deoxidise with 0.3–0.5 % manganese and cast.
  2. Forge and roll to sheet 0.35–1 mm, or strip to 0.05 mm for tape cores.
  3. Form the part completely — bend, weld, drill.
  4. Anneal at 1,050–1,150 °C for 2–4 hours in dry hydrogen or cracked ammonia, cool slowly to about 600 °C, then faster.
  5. Never bend, drop or hammer it afterwards. A knock can halve its permeability.

Uses: microphone and audio transformers, measuring transformers, tape heads (Recording Sound), telephone loading coils, and shields.

Magnetic shields

The field takes the easy path through the wall, around the inside Compass inside barely feels a magnet outside Outer shield soft iron, takes strong fields Seams overlapped 10 mm+ Inner shield mu-metal Gap 1 cm or more Hole as a tube field fades within one diameter
Fig. 3 How a magnetic shield works. The field is not blocked; it is drawn into the easy path of the high-permeability wall and carried round the space inside, which is left almost field-free. Two shields with a gap between them work far better than one thick one.

A shield does not block magnetism like a wall stops wind; it offers an easier path round the space inside. For a long tube, the field inside falls by roughly permeability × wall thickness ÷ diameter: a mu-metal tube 100 mm across with a 1 mm wall and permeability 20,000 cuts it about 200 times. Two shields with a centimetre or more between them multiply their factors.

  1. Material: mu-metal for weak fields; a soft iron or silicon steel layer outside it where the field is strong, so the mu-metal does not saturate.
  2. Closed shape: a cylinder with end caps, or a box with rounded corners.
  3. Seams overlapped at least 10 mm, spot-welded or riveted.
  4. Holes small, and extended outward as short tubes: a hole lets field in about one diameter deep.
  5. Anneal the finished shield in hydrogen; handle gently after.

Copper is not a magnetic shield at steady or mains frequencies; it works only at radio frequencies, by eddy currents. For both, put a copper box inside an iron one. Uses: the necks of cathode-ray tubes (Cathode Rays and Television, oscilloscopes), audio transformer cans, magnetometer rooms, and the walls of an MRI room (Ultrasound, CT and MRI).

How to tell it worked

  • Laminations: clean edges, bulb test passed; the finished core, running with nothing on its secondary, is barely warm after an hour and hums softly or not at all.
  • Comparing cores: put the same 100-turn coil on two cores at the same low AC voltage, secondary open. The better core draws less current and runs cooler.
  • Powder core: a 20-turn coil on it has 10–90 times the inductance of the same coil on a wooden ring (Electronic Test Equipment).
  • Ferrite: black, hard, rings like porcelain, chips glassily; a magnet sticks firmly.
  • The Curie test: stick a small magnet on a piece of ferrite and warm it slowly on a hotplate beside a The Thermometer. At some temperature — 150–250 °C for manganese–zinc, 100–500 °C for nickel–zinc depending on zinc — the magnet drops off. Batches that drop at the same temperature match: the simplest quality control there is.
  • Shield: a The Compass inside barely stirs when a magnet comes within a few centimetres outside; unshielded, it swings at 30 cm.

Note Troubleshooting. Transformer core hot, hums → burrs, thin coating, loose laminations, or too few turns per volt. Relay armature sticks → core not annealed, or carbon in the iron. Ferrite cracks in the kiln → too fast through binder burn-out, or uneven pressing. Ferrite soft, crumbly → under-fired. Magnetic but poor → impurities, wrong proportions, or (manganese–zinc) oxygen while cooling. Powder core hot → grains too coarse or badly insulated. Shield weak → seams not overlapped, bent after annealing, or magnetised: pass it slowly through and away from a coil carrying AC.

Dangers

Danger Hydrogen furnaces. Hydrogen mixed with air explodes. Flush with nitrogen before admitting hydrogen and before opening; burn the exhaust gas; never open a hot box of hydrogen.

Danger Fine iron powder catches fire by itself. Cool freshly reduced powder under hydrogen or nitrogen, then let air in very slowly over hours. Store it closed, away from sparks, and smother fires with dry sand, never water.

  • Dust: nickel, manganese and ferrite powders harm the lungs; nickel causes allergy and, over years, cancer; manganese dust damages nerves. Mill wet, wear a mask, wash.
  • Carbon monoxide and iron carbonyl are deadly: carbonyl iron is for industry only.
  • Power presses take fingers — use guards or two-handed controls; punched laminations cut like razors.

What this unlocks

How it was first done

Michael Faraday wound his first transformer on a solid iron ring in 1831; by the 1880s dynamo and transformer builders cut cores from thin sheet or wire. In 1900 William Barrett, W. Brown and Robert Hadfield published the low losses of silicon steel, which spread into transformer works from about 1903–1906, and Norman Goss patented grain-oriented steel in 1934. At Western Electric, Gustav Elmen discovered permalloy around 1916; it was wrapped round the 1924 New York–Azores telegraph cable to speed it up. Willoughby Smith and Henry Garnett in Britain developed mu-metal in 1923 for the same purpose. Pressed iron-dust cores served telephone loading coils from about 1916, and Hans Vogt's "Ferrocart" iron-powder radio coils appeared in Germany in the early 1930s. Yogoro Kato and Takeshi Takei in Tokyo invented ferrites around 1930, and TDK was founded in 1935 to make them; J. L. Snoek at Philips worked out manganese–zinc and nickel–zinc ferrites during the Second World War, opening the way to compact television transformers, ferrite rod aerials and switch-mode supplies.

Source: content/entries/electricity/magnetic-cores.md