Crack oil and gas into ethylene and propylene, join those small molecules into the long chains of polyethylene, polypropylene, PVC, polystyrene and PET, and melt them into pipes, bags, bottles and moulded parts by the million. How each plastic is made, how to tell them apart, how a workshop can extrude, mould and blow them, why the chemical plants need a whole industry — and how to recycle what you have.

Difficulty
●●●●●
Time
Days to set up a hand injection press or small extruder; years and a chemical industry for a polymer plant
Steps from zero
26 prerequisites →

You need first

Early PlasticsPetroleum and Refining

This unlocks

Membranes, Reverse Osmosis and Desalination
The full path from nothing — 26 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. Pottery
  10. The Kiln
  11. Charcoal
  12. Hides and Leather
  13. Lime
  14. Lye and Potash
  15. Fermentation
  16. Glass
  17. Bellows
  18. Saltpeter
  19. Distillation
  20. Iron (the Bloomery)
  21. Sulfuric Acid
  22. Blacksmithing
  23. Nitric Acid
  24. Steel
  25. Early Plastics
  26. Petroleum and Refining
  27. Petrochemicals and Modern Plastics

Do them roughly in this order. See it on the tech tree →

Why it matters

Look around any modern home and much of what you see is plastic: pipes, wire insulation, buckets, bottles, bags, toothbrushes, toys, the cases of every electrical thing. It is cheap because it is made from the light fractions of Petroleum and Refining and Natural Gas and Helium by the million tonnes, then melted and shaped in seconds by machines.

It matters most where nothing else does as well. A polyethylene pipe carries clean water for fifty years without rusting (Pipes, Plumbing and Aqueducts). Plastic sheet keeps grain dry (Granaries and Food Storage) and covers greenhouses (Cold Frames, Cloches and Greenhouses). Plastic syringes, drip bags and gloves made medicine cheap and sterile (Syringes and Hypodermic Needles, Intravenous Fluids), and plastic insulation made wiring safe (Wiring and Electrical Safety).

Be honest about what is realistic. Shaping plastics is a workshop craft: a small community can extrude pipe, mould parts and blow bottles. Making plastics from oil is not: it needs chemical plants working at hundreds of degrees and, for some, a thousand times atmospheric pressure, run day and night by trained crews. Meanwhile the world after any collapse will be full of old plastic — raw material and lasting nuisance at once. So: understand plastics, sort and reshape what exists, then build the chemistry.

How it works

Long chains

Every plastic is made of polymers: molecules thousands of atoms long, built by joining small molecules called monomers end to end, like beads on a string (Early Plastics explains the idea with shellac and Bakelite). The long chains tangle like cooked spaghetti, which is what makes plastic tough instead of brittle.

Most plastics are made from monomers containing a double bond — two carbon atoms joined twice. Open it, and each carbon has a free hand to grab the next monomer. Started by a trace of a reactive chemical (an initiator) or on the surface of a catalyst, a chain grows by thousands of links in a fraction of a second. Ethylene (two carbons and four hydrogens) gives polyethylene. Replace one hydrogen with a carbon and you have propylene, giving polypropylene; with chlorine, vinyl chloride, giving PVC; with a benzene ring, styrene, giving polystyrene. PET is different: it is made, like nylon, by joining two different molecules that give off water each time they link (Rayon and Nylon).

All of these are thermoplastics: they soften when heated and harden when cooled, again and again. That is why they can be shaped in seconds and recycled. Bakelite and other thermosets set once, for ever (Early Plastics, Resins: Phenolic, Polyester and Epoxy).

The common plastics

Code Plastic Density (water = 1) Softens / melts Shaped at Typical uses
1 PET (polyethylene terephthalate) 1.38 — sinks Melts 250–260 °C 270–290 °C, dried first Drinks bottles, food trays, polyester fibre
2 HDPE (high-density polyethylene) 0.95 — floats Melts 130–135 °C 180–240 °C Water pipe, milk jugs, buckets, crates, thin crinkly bags
3 PVC (polyvinyl chloride) 1.35–1.45 — sinks Softens 75–85 °C 160–200 °C, with stabiliser Drain and water pipe, window frames, cable covering, soft tubing
4 LDPE (low-density polyethylene) 0.92 — floats Melts 105–115 °C 160–220 °C Soft film, bags, squeeze bottles, cable insulation
5 PP (polypropylene) 0.90 — floats Melts 160–165 °C 200–250 °C Caps, hinged boxes, rope, car parts, medical syringes
6 PS (polystyrene) 1.05 — just sinks Softens about 95 °C 180–240 °C Clear brittle cups, cutlery, foam packing and cups

The number in a small triangle moulded into most plastic goods is this code.

Making the monomers: cracking

Ethane from natural gas Naphthafrom crude oil Steam Cracking furnace 750–875 °C for under half a second, in tubes Quench chill at once Compress wash, dry, chill to −150 °C Ethylene → PE, PVC, PS, PET Propylene → PP Others butadiene, benzene, fuel columns separate the gases Without oil: alcohol from sugar vapour over hot alumina, 350–450 °C, gives ethylene and water
Fig. 1 From oil and gas to pellets. Ethane or naphtha is mixed with steam and heated to about 850 °C for a fraction of a second in tubes inside a furnace, then chilled at once. The cracked gas is compressed, dried and cooled far below freezing so that a train of columns can boil off ethylene, propylene and the rest. Each monomer goes to its own reactor and comes out as pellets.

Ethylene and propylene do not occur in nature in useful amounts. They are made by steam cracking: breaking bigger hydrocarbon molecules apart with heat.

  1. Feed. Ethane, separated from Natural Gas and Helium, or naphtha, the light petrol fraction from distilling crude oil (Petroleum and Refining, Distillation).
  2. Crack. The feed is mixed with steam (which keeps the molecules apart and slows soot formation) and blown through 10–15 cm alloy-steel tubes hanging in a gas-fired furnace, reaching 750–875 °C for 0.1–0.5 seconds. The heat snaps carbon–carbon and carbon–hydrogen bonds and leaves double bonds behind.
  3. Quench. Within milliseconds the gas is chilled to about 400 °C in heat exchangers that raise steam, or the useful molecules would go on reacting into tar and coke.
  4. Separate. The gas is compressed to about 35 bar, washed with caustic soda (Lye and Potash) to remove sulfur and carbon dioxide, dried, then cooled as low as −150 °C (Ice and Refrigeration, Liquid Air, Nitrogen and the Noble Gases) and distilled in a train of tall columns. Ethylene boils at −104 °C and propylene at −48 °C, so each comes off in its own column.

From ethane, about three-quarters becomes ethylene. From naphtha, about a third becomes ethylene, a sixth propylene, and the rest butadiene (for Synthetic Rubber Works (Overview)), benzene (for styrene and nylon) and fuel.

The other monomers. Vinyl chloride is made by adding chlorine to ethylene and cracking the product to strip off hydrogen chloride; the chlorine comes from salt by Electrolysis (Chlorine and Bleach, Salt). PVC is 57% chlorine by weight, so more than half of it comes from salt, not oil. (An older route joined acetylene from carbide with Hydrochloric Acid over a poisonous mercury catalyst.) Styrene comes from ethylene and benzene (Coal Tar Chemicals); the raw materials of PET from ethylene and from an oil hydrocarbon called para-xylene.

Ethylene without oil

Ethylene can also be made from alcohol. Pass ethyl alcohol vapour (Fermentation, Distillation) over a bed of alumina (aluminium oxide, from bauxite — see Aluminium) heated to 350–450 °C, and each alcohol molecule loses a molecule of water and becomes ethylene, with 95% or better yield. It takes about 1.7 kg of pure alcohol per kilogram of ethylene — about 3.5 kg of sugar, or 25–30 kg of sugarcane. Brazil makes polyethylene this way from sugarcane today, and India did in the 1960s. For a society without oil, it is the most achievable route to ethylene — a steel tube of catalyst in a furnace, a condenser and a gas holder. Turning the gas into polymer is the hard part.

Making the polymers (in outline)

These are chemical-plant processes. They are given so a rebuilding society knows what to aim for, not as bench experiments.

  • LDPE — ethylene compressed to 1,000–3,000 bar and heated to 150–300 °C with a trace of oxygen or peroxide. The chains grow branched and pack loosely: soft, clear, low density. The compressors and thick-walled reactors are among the most demanding machines in industry.
  • HDPE and PP — made at only 10–40 bar and 50–110 °C on a catalyst: either titanium chloride with an aluminium compound (the Ziegler–Natta catalysts) or chromium oxide on silica (the Phillips catalyst). The chains grow straight from the catalyst and pack tightly: stiffer, stronger, higher-melting. For polypropylene the catalyst also lines up every side group the same way; without that you get a sticky goo. The catalysts are ruined by traces of water and air, and the aluminium compounds catch fire in air.
  • PVC — liquid vinyl chloride (it boils at −13 °C, so it is kept under a few bar of pressure) is stirred in hot water at 50–70 °C with an initiator, in droplets; each droplet becomes a grain of PVC powder. The leftover vinyl chloride must be stripped out completely: it causes a rare liver cancer, discovered in factory workers in 1974. PVC powder is then mixed with heat stabilisers (it otherwise gives off hydrogen chloride when heated) and, for soft PVC, up to 40% of an oily plasticiser.
  • Polystyrene — styrene heated to 100–150 °C polymerises by itself; the leftover styrene is boiled off.
  • PET — terephthalic acid and ethylene glycol heated to 250–290 °C, finally under strong vacuum (The Vacuum Pump) with an antimony catalyst to draw off glycol and lengthen the chains.

Every plant ends the same way: the molten polymer is squeezed through holes into strands, cooled in water and chopped into pellets 3–5 mm long, the form in which plastic is shipped to the shaping factories.

Shaping plastics in the workshop

This is the part a community can do. Start with clean, sorted plastic of a single kind.

Sorting: tell the plastics apart

  1. Read the code if there is one.
  2. Float test. In water, PE and PP float; PS, PVC and PET sink. In water mixed with an equal volume of strong alcohol (density about 0.93), PP still floats and most PE sinks. In strong brine (as much Salt as will dissolve, density about 1.2), PS floats and PVC and PET sink.
  3. Burn test — a small sliver held in tongs in a flame, outdoors:
    • PE: blue flame with a yellow tip, drips burning, keeps burning, smells of candle wax.
    • PP: similar, with a sharper, oilier smell.
    • PS: yellow flame with thick black soot, sweet flowery smell.
    • PET: yellow, sooty, drips, often goes out by itself.
    • PVC: hard to light, goes out when taken from the flame, green edge to the flame, sharp acid smell. Confirm with the copper wire test: heat a copper wire red, touch it to the sample, put it back in the flame; a bright green flame means chlorine. Do not breathe the fumes.
  4. Wash, dry and cut or grind into pieces 5–10 mm across.

PE and PP are the easiest to work: they melt gently, do not need drying, and give off little smoke. Begin with them.

Pressing

The simplest shaping is the hot press of Early Plastics: PE or PP chips in a greased mould, melted in an oven at 180–200 °C, then pressed and cooled under load — for sheets, chopping boards, washers and handles. Sheet can be welded with a stream of hot air and a filler rod of the same plastic.

The extruder

motor, gears Heater bands hotter towards the die Hopper Screen Die feed deep channel compression melts and squeezes metering shallow, pumps Making pipe ring die sizing sleeve water bath, metres long haul-off saw Making film frost line air ring rollers flatten ring die, pointing up bubble
Fig. 2 Above: a screw extruder. Pellets fall from the hopper onto a turning screw in a heated barrel; the screw's channel gets shallower along its length, so the plastic is squeezed, melted by heat and friction, and pumped through a mesh screen into the die. Below: two ways to use it. A ring-shaped die makes pipe, which is sized and cooled in a water bath and pulled away at steady speed; or the tube is blown up into a thin bubble and flattened between rollers to make film for bags.

An extruder is the machine behind pipe, film, wire insulation, rods, sheet and the pellets themselves. It is a screw turning in a heated barrel, like a meat mincer:

  • Barrel: a thick steel tube bored true (Drills and Boring), 20–60 mm bore and 15–30 times as long, wrapped with nichrome heater coils (Electric Kettles, Irons, Heaters and Cookers) in three or four zones, each with its own control (Thermostats and Automatic Control), hotter towards the die — for HDPE about 170, 190, 210 °C.
  • Screw: cut on a lathe like a long lead screw (Screws, Nuts and Bolts), with a deep channel at the hopper end, a tapering compression section, and a shallow metering section at the end, about one-third as deep. This squeezes out air and builds pressure. Clearance to the barrel: about 0.1–0.2 mm. A workshop shortcut that works for a first machine is a large wood-auger bit turning in a close-fitting steel pipe.
  • Drive: an The Electric Motor and reduction Gears to 20–60 turns a minute, with a thrust bearing behind the screw (Making Ball and Roller Bearings). The feed throat is water-cooled so pellets do not stick before reaching the screw.
  • Screen: fine wire mesh on a perforated steel plate catches dirt before the die. Change it often with recycled plastic.

A 25 mm workshop extruder pushes out 2–8 kg of plastic an hour.

Plastic pipe

A plastic pipe is extruded through a ring-shaped die: an outer ring and a central mandrel held by thin spokes, which the melt flows around and rejoins. The soft tube is drawn into a sizing sleeve under slight vacuum or internal air pressure, which sets the outside diameter, then through a water bath several metres long, and pulled away by a pair of belts or rollers at steady speed (the haul-off). Faster haul-off makes a thinner wall. Pipe is cut to length — 6 m is usual — or coiled.

  • Sizes. Pipes are named by outside diameter: 20, 25 and 32 mm for house supply, 50–110 mm for mains and drains. The wall is set by the SDR — diameter ÷ wall. HDPE water pipe of SDR 11 (a 32 mm pipe with a 2.9 mm wall) takes 10–16 bar, depending on the grade of polyethylene. Drain pipe needs much thinner walls.
  • Black for sunlight. Sunlight makes polyethylene brittle in one or two summers. Mixing in 2–3% fine Lampblack and Carbon Black (soot) protects it for decades; that is why water pipe is black.
  • Joining. PE pipe is joined by butt fusion: the square-cut ends are pressed against a hot plate at about 220 °C until a small bead forms, the plate is removed, and the ends are pressed together and held until cool. A good joint is stronger than the pipe. PVC is joined with solvent cement — PVC dissolved in a strong solvent (Ether, Acetone and Solvents) — painted on a spigot and pushed into a socket; the two surfaces dissolve into each other and harden.
  • Good and bad. A good pipe is round, with the wall even all round (calipers at four points, Measurement from Scratch) and glossy inside and out; rough, matt or bubbly surfaces mean cold, wet or dirty plastic.

Plastic bags and film

A plastic bag starts as blown film. A ring die points upwards; the tube of melt rising from it is blown up with a little air from inside into a bubble two to four times the die's diameter, stretching it thin in both directions. A ring of air cools it; you can see the frost line where clear melt turns hazy solid. At the top, guide boards and a pair of rollers flatten the bubble into a double layer and pull it up at steady speed. The flat tube is sealed across with a hot bar at 120–160 °C and cut into bags.

Thin crinkly carrier bags are HDPE about 15–20 thousandths of a millimetre (micrometres) thick; soft bags and sheeting are LDPE, 30–150 micrometres. Good film is even, without lines, holes or gel lumps. In the workshop, seal film with a hot iron through baking paper, or a heated nichrome wire.

The injection mould and moulding machine

Injection mould (closed) Nozzle Sprue Cavity Runner, gate Cooling water Ejector pins fixed half above, moving half below; they part along the dashed line and the pins push the parts off. Stretch-blow moulding a bottle 1 Preform warmed to 95–110 °C 2 Stretch a rod pulls it long and thin 3 Blow air at 25–40 bar, cold mould sets it The thread is moulded first and never stretched.
Fig. 3 Left: an injection mould, closed. Melt enters through the sprue, runs along the runner and through a small gate into the cavity. Water channels cool the steel; vents let air out; ejector pins push the cold part off the core when the mould opens. Right: making a bottle by stretch-blow moulding. A test-tube-shaped preform is warmed, a rod stretches it downwards, and air at 25–40 bar blows it out against the cold walls of the bottle mould.

An injection moulding machine heats plastic in a barrel and forces it into a closed, cold mould, where it sets in seconds. Every cap, bucket, comb, crate and syringe barrel is made this way. The industrial machine uses a screw that both melts the plastic and then rams forward like a plunger, at 500–1,500 bar; a hydraulic or toggle clamp holds the mould shut with tens to thousands of tonnes (Hydraulic Presses and Rams).

A workshop plunger machine is simpler: a steel barrel of 20–25 mm bore and about 20 cm long, wrapped with a 300–500 W heater band and a thermometer, a nozzle 3–4 mm across at the bottom, and a close-fitting plunger pushed down by a long lever (10 to 1 or more) or a screw. The mould is clamped under the nozzle. With 50 kg on a lever of 10 to 1, the pressure is about 100 bar — enough for small, chunky parts of PE, PP or PS up to 20–40 g: knobs, washers, caps, toy parts.

The injection mould is the costly part, and its design decides everything:

  • Two halves, a cavity and a core, meeting at a parting line, aligned by hardened guide pins. Industrial moulds are hardened tool steel (Alloy and Stainless Steels) and last millions of shots; workshop moulds of Aluminium or brass, milled on Machine Tools, last thousands.
  • Sprue, runner and gate. Melt enters through a tapered sprue, flows along runners, and enters the cavity through a small gate, about half the part's wall thickness, so the runner snaps off cleanly.
  • Vents — tiny slots 0.02–0.04 mm deep at the far end of the cavity — let trapped air escape. Without them the part is short or scorched.
  • Draft: every wall tapers 1–2° so the part comes off (Early Plastics).
  • Shrinkage: the part shrinks as it cools, so the cavity is made larger — about 2% for PE, 1.5% for PP, 0.5% for PS.
  • Even walls of 1–3 mm; thick spots sink and leave hollows. Ribs, not solid lumps, give stiffness.
  • Cooling channels 8–12 mm bore drilled through the steel near the cavity, with water running through.
  • Ejector pins that push the part off the core when the mould opens.

A good part is fully filled, sharp-cornered, free of bubbles and sink marks, with only a hair-thin flash at the parting line.

The plastic bottle

A plastic bottle is blown, like Glass, but cold moulds and stretching let it be astonishingly thin.

  • Extrusion blow moulding (HDPE milk jugs, detergent bottles, canisters): an extruder pushes out a soft tube downwards (the parison); a two-part mould closes on it, pinching and sealing the bottom; air at 5–10 bar blows it out against the cold walls; the mould opens and the waste at top and bottom is trimmed. A workshop can do it with a small extruder, a split aluminium mould and a pump at 2–6 bar (Bellows to Air Compressors).
  • Stretch blow moulding (PET drinks bottles): first, a preform like a thick test tube, with the screw thread already finished, is injection-moulded. It is reheated by infrared lamps to 95–110 °C — soft but not melted — placed in a bottle mould, stretched lengthwise by a rod, and blown at 25–40 bar against the chilled mould. Stretching in both directions lines up the chains and makes the thin wall strong and gas-tight. A 500 ml bottle weighs 10–20 g; a carbonated drinks bottle holds 3–4 bar of fizz and bursts well above 10 bar; the five-lobed "petaloid" base stops it bulging.

A good bottle has an even wall (look at it against a light — thin spots show), stands upright, and its thread takes a cap tightly. A bottle for pressure is tested by filling with water and pumping it to twice its working pressure.

Recycling

Recycling thermoplastics is easy in principle: sort, wash, melt, shape (Rubbish, Recycling and Reuse). In practice:

  1. Sort strictly. Different plastics do not mix when melted; a few percent of PVC in PE spoils it, and PVC decomposes at the temperatures PET needs.
  2. Wash off food, oil and labels in hot water with Soap or washing soda; dry.
  3. Grind to flakes 5–10 mm across. Dry PET for about 4 hours at 150–160 °C before melting, or it breaks down and goes brittle.
  4. Re-extrude through a fine screen to catch dirt, into strands cooled in water and chopped into pellets.

Each melting shortens the chains a little, so recycled plastic suits thicker goods — drain pipe, crates, posts, buckets — or is mixed with new.

Polyethylene and polypropylene that cannot be reused burn hot — about as much heat per kilogram as fuel oil — and fairly cleanly in a hot, well-aired furnace (Boilers and Pressure Vessels). Never burn PVC: see below.

How to tell it worked

  • Pellets and sheet are even in colour, without black specks (burnt) or bubbles (wet).
  • Pipe, capped and full of water, holds 1.5 times its working pressure for an hour without leaking or swelling; a short ring crushed flat in a vice springs back without cracking.
  • Bags stretch long before tearing; seals peel only by tearing the film beside them.
  • Moulded parts fill completely and come out without sticking.
  • Bottles hold twice their working pressure.

Note Troubleshooting. Bubbles, silvery streaks: wet plastic — dry it. Black specks, smoke, acid smell: too hot or held too long, or PVC mixed in. Part not filled: too cold, too little pressure, gate too small, or no vents. Part sticks: not enough draft or mould too hot. Sink marks: walls too thick, or not held under pressure while cooling. Extruder surging (output pulses): feed bridging in the throat — keep it cool; or screw slipping on a too-hot barrel at the feed end. Brittle product: overheated, sunlight-damaged, or too much recycled material.

Dangers

Danger Burning and overheated PVC gives off hydrogen chloride, which forms hydrochloric acid in the lungs, and dioxins, which are long-lasting poisons. Never burn PVC, never heat it above about 200 °C, and work with it only with strong ventilation. Polystyrene fumes contain styrene, an irritant and probable carcinogen.

Danger Monomers and plants. Ethylene and propylene are colourless gases that explode when mixed with air at as little as 2–3%. Vinyl chloride causes liver cancer. Polymerisations release heat and can run away. Polymer plants need pressure-rated vessels, relief valves, gas detectors and trained crews — not a shed.

  • Molten plastic sticks to skin and keeps burning; it is hotter than boiling water by 100 °C or more. Wear gloves, long sleeves and a face shield near the nozzle and die; never look into the barrel or hopper of a hot machine.
  • Trapped pressure. A blocked nozzle can blow molten plastic out when it clears: heat the nozzle first and never stand in front of it. Moulds and clamps close with tonnes of force: guard them.
  • Plastic litter lasts for centuries, breaks into tiny pieces that animals eat, and blocks drains. Collect, sort and reuse; do not dump or burn in the open.

What this unlocks

Cheap water pipe and drainage (Pipes, Plumbing and Aqueducts, Sewers and Wastewater), film for farming and food storage, insulated wire, sterile single-use medical goods, Rayon and Nylon (PET and polypropylene fibre), plastic housings for electronics, the clear plastic of Flat Screens: LCD and LED Displays, the light parts of Electric Vehicles and aircraft, and the cheap filament of 3D printers, which melt plastic and lay it down a line at a time.

How it was first done

Polystyrene was first noticed in 1839 by the German apothecary Eduard Simon, who distilled styrene from a tree resin and found it set into a jelly; it was made commercially by IG Farben in Germany from 1931. PVC was patented by Fritz Klatte in Germany in 1913; Waldo Semon in the United States made it flexible with a plasticiser in 1926. Polyethylene was discovered by accident at ICI in England on 27 March 1933, when Eric Fawcett and Reginald Gibson heated ethylene to about 1,400 bar and found a waxy white solid — a trace of leaked-in oxygen had started it. Production began in 1939, and its first great use was insulating the cables of wartime radar (Radar and Microwaves).

In 1951 Paul Hogan and Robert Banks at Phillips Petroleum found the chromium catalyst for HDPE; in 1953 Karl Ziegler in Germany found titanium catalysts that made it at near-normal pressure, and in 1954 Giulio Natta in Italy used them to make useful polypropylene; the two shared the Nobel Prize in 1963. PET was invented by John Whinfield and James Dickson in Manchester in 1941, and the stretch-blown PET bottle was patented by Nathaniel Wyeth at DuPont in 1973. World plastics production grew from almost nothing in 1950 to around 400 million tonnes a year in the 2020s.