Calcium Carbide and Acetylene
Bake lime and coke together in an electric arc and you get calcium carbide — a grey stone that fizzes in water and gives off acetylene, a gas that burns with a brilliant white light and, with oxygen, the hottest flame in common use. Carbide gives lamps, welding, nitrogen fertiliser and a whole branch of chemistry.
- Difficulty
- ●●●●●
- Time
- A day per furnace run once the arc furnace works; an afternoon to make a lamp
- Steps from zero
- 25 prerequisites →
The full path from nothing — 25 steps before this one
- Fire
- Cordage and Rope
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Hunting and Trapping
- Basic Woodworking
- Charcoal
- Pottery
- The Kiln
- Hides and Leather
- Bricks
- Lime
- The Wheel and Axle
- Firebrick and Refractories
- Bellows
- Gears
- Iron (the Bloomery)
- Copper Smelting
- The Waterwheel
- Blacksmithing
- Magnets
- Copper Wire
- The Generator
- The Electric Arc Furnace
- Calcium Carbide and Acetylene
Do them roughly in this order. See it on the tech tree →
Why it matters
Calcium carbide is light, heat and chemistry packed into a stone. Kept dry in a tin, it lasts for years. Drop it into water and it gives off acetylene, a gas that:
- burns with a pure white light, many times brighter than an oil lamp for the same size of flame. Carbide lamps lit mines, bicycles, carriages, lighthouses and whole villages before electric light reached them (Lamps and Candles, The Light Bulb);
- burns with oxygen at about 3,100 °C, hot enough to weld and cut steel (Welding);
- is the starting point for acetic acid, plastics and synthetic rubber — a whole chemical industry built on coal, lime and electricity, with no oil at all (Early Plastics, Synthetic Rubber Works (Overview)).
Heated in nitrogen, carbide also takes nitrogen out of the air to make calcium cyanamide, a fertiliser — the first industrial way to fix nitrogen, years before ammonia synthesis (Chemical Fertilisers, Ammonia).
The cost is electricity: about 3–4 kWh for every kilogram of carbide in a good furnace, more in a small one. Where you have water power (Water Turbines and Hydroelectric Power) and limestone, carbide is one of the best uses for it.
How it works
- Making it. At about 2,000–2,200 °C — far beyond any fuel-fired furnace, so only the electric arc will do (The Electric Arc Furnace) — carbon pulls the oxygen off quicklime and also joins with the calcium: quicklime + coke → calcium carbide + carbon monoxide (CaO + 3 C → CaC₂ + CO). The carbon monoxide burns at the top of the furnace with blue flames.
- Using it. Carbide reacts with water at once: calcium carbide + water → acetylene + slaked lime (CaC₂ + 2 H₂O → C₂H₂ + Ca(OH)₂). The reaction makes a lot of heat. The lime is left behind as a wet grey-white sludge.
- Why acetylene is special. Its two carbon atoms are joined by a very strong triple bond that holds a lot of stored energy. When it burns, that extra energy makes the flame hotter than any other common fuel gas, and tiny glowing carbon particles in the flame make it shine white. The same stored energy makes it unstable: squeezed above about 1 bar above atmospheric pressure, it can break down explosively on its own, without any air.
Numbers worth remembering:
| Gas from 1 kg of good commercial carbide | about 280–300 litres of acetylene (pure carbide would give 350) |
| Slaked lime left over | about 1.2 kg (dry weight) per kg of carbide |
| Water for a cool reaction | at least 8 litres per kg of carbide in a generator |
| Burns in air when mixed at | anywhere from 2.5% to over 80% acetylene — an enormously wide explosive range |
| Electricity to make 1 kg | 3–4 kWh in a large furnace; 5–10 kWh in a small one |
What you need
| Item | Amount | Notes |
|---|---|---|
| An electric arc furnace with a carbon-lined hearth | 1 | See The Electric Arc Furnace. A small one of 20–50 kW makes a few kilograms an hour. |
| Quicklime, freshly burned | 60 parts by weight | Burn the purest limestone you have, low in clay and magnesia (Lime). Lumps 1–5 cm. |
| Coke or hard charcoal | 40 parts by weight | Low in ash and sulfur (Coal and Coke, Charcoal). Lumps 1–5 cm. |
| Iron pans or a heavy iron box | — | To tap into or to hold the cooled ingot |
| Airtight iron drums or tins | — | Carbide must never get damp |
| Sledgehammer, goggles, leather gloves | — | For breaking carbide |
For lamps: thin sheet brass or tinplate (Sheet Metal and Rolling, Soldering and Brazing), a small screw valve, felt, and a burner tip — traditionally of soapstone (steatite), which does not clog or overheat.
Where to find it
- Limestone: pale grey or white rock that fizzes with vinegar (Lime, Rocks and Minerals). For carbide, choose the purest: the whitest stone, giving the whitest, most powdery quicklime. Phosphate in the lime turns into poisonous phosphine gas in the acetylene; magnesia makes a sticky charge.
- Coke: baked from coal (Coal and Coke). Hard charcoal from dense hardwood also works, but it crushes more easily and burns away at the top of the charge.
Method 1: Making carbide
The arc furnace and its electrical side are described in The Electric Arc Furnace (Ferroalloys, calcium carbide and silicon). The simplest small-scale way is the ingot (block) method used by the first carbide makers:
- Dry everything. Burn the lime the day before and keep it hot or sealed; damp lime makes steam and spatters. Crush lime and coke to 1–5 cm, sieve out the dust (dust chokes the gas flow), and mix them 60 : 40 by weight.
- Start the arc on a bed of coke in the carbon-lined hearth, with the electrode lowered almost to touching.
- Feed the charge around the electrode so it is buried. Carbon monoxide flames up through the charge in bluish tongues. Keep adding charge as it sinks.
- Raise the electrode slowly as a pool of liquid carbide builds up under it. The pool is grey-black, thick, and about 2,000 °C — too bright to look at without dark welding glass.
- After several hours, switch off. Leave the block to cool at least overnight under its crust of unreacted charge.
- Break it out. The block is a lump of grey, crystalline carbide wrapped in a crust of half-reacted lime and coke. Knock off the crust (put it back into the next charge) and break the carbide into pieces, wearing goggles: chips fly.
- Grade and store. Sieve into sizes — 1–2 cm ("nut") for lamps, 2–8 cm for generators — and seal at once in airtight iron drums or soldered tins. Label them.
Larger furnaces are tapped every one to two hours instead: the liquid carbide runs out of a taphole into iron pans.
Tip Test your carbide. Fill a jar or bottle of known size with water, turn it upside down in a basin of water, and drop 10 g of carbide in a little cloth bag under its mouth. Good carbide fills about 2.8–3 litres with gas. Less than 2 litres means much unreacted lime or coke: raise the coke slightly, or run hotter and longer.
Method 2: The carbide lamp
A carbide lamp is a tiny water-to-carbide gas generator with a burner on top. Miners' cap lamps, bicycle lamps and house lamps all work the same way.
- The carbide chamber. A screw-on cup of brass or tinplate, about 5–6 cm across and 5 cm deep for a hand or cap lamp. Fill it no more than half with nut-sized carbide (about 50–60 g): carbide swells as it turns into lime and will jam the lamp if overfilled.
- The water tank above it, with a filling cap. A needle valve (a tapered pin in a small hole, raised and lowered by a lever or screw) lets water drip through a tube onto the carbide.
- The filter. A felt or cotton pad where the gas leaves the chamber catches lime dust and moisture.
- The burner tip. A tiny hole, about 0.3–0.5 mm, drilled in a soapstone or brass tip. Better tips have two small jets angled to meet: the streams flatten each other into a broad fan-shaped flame and draw in air, so they burn without soot.
- The reflector. A polished concave dish of brass or tinned sheet behind the flame throws the light forward.
Using it. Fill the tank with water and the chamber half with carbide, screw it tight, open the valve two or three clicks, wait 10–20 seconds for the gas to push out the air, and then light the jet with a spark or match (Matches). Adjust the drip for a flame 2–3 cm long. A charge of 50–60 g lasts 3–4 hours, giving the light of several candles. When the flame weakens, add more water; when water no longer helps, the carbide is spent — empty the grey lime sludge outdoors and recharge.
House lighting. For a building, use a larger generator outside (see Welding for the carbide-to-water generator and floating gasholder), and pipe the gas indoors through iron pipe to burners of 15–30 litres an hour, each as bright as 25–50 candles. Never put the generator inside a house.
Method 3: Acetylene as a chemical
These are industrial processes, given in outline so you know where carbide leads:
- Welding and cutting. Acetylene with oxygen (Hydrogen, Oxygen and Gases) — see Welding. For transport, acetylene is dissolved in acetone (Ether, Acetone and Solvents) soaked into a porous filling inside a steel cylinder: acetone holds about 25 times its own volume of acetylene for each bar of pressure, and the filling keeps any decomposition from spreading.
- Acetaldehyde and acetic acid. Acetylene bubbled into warm dilute Sulfuric Acid containing a mercury salt as a helper (catalyst) takes up water and becomes acetaldehyde; blown with air, that becomes pure, strong acetic acid — far stronger than vinegar, for dyes, medicines and acetate. This process poisoned Minamata Bay in Japan with mercury in the 1950s: the mercury waste must never reach water (Mercury).
- Vinyl chloride and PVC. Acetylene with hydrogen chloride over a mercury catalyst gives vinyl chloride, which can be joined into the plastic PVC.
- Synthetic rubber. Acetylene can be built up into neoprene and other synthetic rubbers (Synthetic Rubber Works (Overview)).
- Calcium cyanamide (nitrolime). Crushed carbide heated to about 1,000–1,100 °C in a stream of nitrogen takes it up and becomes a black powder of calcium cyanamide and carbon. Nitrogen can be made by passing air slowly over red-hot copper turnings, which take out the oxygen. Spread on fields a couple of weeks before sowing, cyanamide is both a nitrogen fertiliser and a weed killer; boiled with water under pressure it gives off Ammonia, and it is the road to melamine plastics. Cyanamide dust is poisonous, and anyone who has breathed it and then drinks alcohol becomes violently sick. See Chemical Fertilisers and Calcium Cyanamide, Dicyandiamide and Melamine.
- Carbide lime. The spent sludge is slaked lime. Settled and drained, it makes good mortar and whitewash (Mortar and Concrete) — but not for treating drinking water or food, because of impurities.
How to tell it worked
- Good carbide is grey to grey-brown, crystalline on fresh breaks, and heavy. A lump dropped in water fizzes hard at once, the water turns milky, and the gas burns with a bright, sooty yellow-white flame.
- Smell. Acetylene itself has only a faint sweetish smell; the strong garlic smell comes from phosphine and other impurities. A very strong smell means impure lime.
- The lamp gives a steady, white, fan-shaped flame without smoke, and does not hiss or flutter.
Note Troubleshooting. Carbide gives little gas → too little carbon, furnace too cool, or it got damp in storage. Seal it better; adjust the charge. Sticky charge that won't sink; electrode rides up → too much carbon or too much dust. Sieve the charge; reduce the coke slightly. Lamp flame jumps and sputters → water dripping too fast or tip partly blocked. Close the valve a little; clean the tip with a fine wire. Lamp smokes → too much gas for the tip, or a single-hole tip. Turn the drip down; use a twin-jet tip. Flame dies after a few minutes though carbide remains → the carbide is caked with lime. Use larger lumps, and do not overfill.
Dangers
Danger Acetylene explodes. Mixed with air in almost any proportion from 2.5% upwards it explodes from a spark. Compressed above about 1 bar gauge it can explode with no air and no spark at all. Never compress acetylene into an empty tank; keep homemade systems at very low pressure (welding systems below 0.1 bar, see Welding). Never let it touch copper, silver or mercury or alloys rich in them: it forms compounds with them that explode when knocked or dried.
Danger Carbide and water in a closed space. A sealed tin of carbide that gets wet bursts like a bomb and fills the room with explosive gas. A flooded carbide store is a disaster. Store carbide in airtight, labelled iron drums, raised off the floor, under a good roof, away from living spaces. Open drums with non-sparking tools (wood, brass). Never put water on a carbide fire: smother it with dry sand.
- Poisonous impurities. Phosphine and hydrogen sulfide in crude acetylene are toxic, and phosphine can set the gas alight on its own. Use pure lime; vent generators outdoors; in a lamp, a little is harmless, but never breathe gas from a generator.
- Caustic lime. Carbide dust and the spent sludge burn eyes and skin like quicklime (Lime). Wear goggles when breaking carbide. Flush eyes with plenty of water for 15 minutes.
- The furnace. All the hazards of the The Electric Arc Furnace: electric shock, the blinding arc, molten carbide at 2,000 °C, and carbon monoxide from the top of the charge.
- Mercury in the chemical processes poisons rivers and people for generations (Mercury).
What this unlocks
- Bright portable light for mines (Mining and Tunnelling), vehicles and homes before electric lamps.
- Gas welding and cutting of steel (Welding) — and with it boilers, ships and machines (The Steam Engine, Steamships).
- Nitrogen fertiliser from the air (Chemical Fertilisers).
- Acetic acid, acetone and plastics (Ether, Acetone and Solvents, Early Plastics).
- Lighthouses and buoys that run unattended for months (Harbours and Lighthouses, Navigation).
How it was first done
Edmund Davy, a chemistry professor in Ireland, discovered acetylene in 1836 by putting water on a potassium compound he had made by accident. Marcellin Berthelot in France named it in 1860, and in 1862 made it directly from carbon and hydrogen in an electric arc. In 1862 Friedrich Wöhler in Germany made calcium carbide and showed that water released acetylene from it — but it was a laboratory curiosity, because nobody could make carbide cheaply.
That changed in May 1892 at Spray, North Carolina. The Canadian inventor Thomas Willson was trying to make calcium metal in an electric furnace from lime and coal tar; instead he got a brittle grey mass that, thrown into a stream, gave off a gas that burned with a sooty, brilliant flame. In the same year Henri Moissan in Paris made carbide in his own arc furnace. Within a few years carbide was made by the hundred tonne at Niagara Falls and in the Alps, and acetylene lamps lit towns and bicycles. In 1895 Henry Le Chatelier showed that the oxygen-acetylene flame was the hottest known, and in 1903 Edmond Fouché and Charles Picard built the first practical welding torch. Georges Claude and Albert Hess found how to store acetylene dissolved in acetone in 1896–97. In 1898 Adolph Frank and Nikodem Caro made calcium cyanamide, the first fertiliser from atmospheric nitrogen. The Swedish engineer Gustaf Dalén won the 1912 Nobel Prize in Physics for automatic acetylene lighthouses with a "sun valve" that turned the light off by day. Miners and cave explorers used carbide cap lamps well into the late twentieth century.
Source: content/entries/chemistry/carbide-and-acetylene.md