◆ Rebuild

Part 7 · Home and Daily Life

Horn and Bone Working

Horn goes soft in boiling water and can be pressed flat, moulded into spoons and cups, split into see-through lantern panes and cut into buttons and handles. Bone and antler are harder and stiffer, the stuff of awls, toggles, handles, buttons and hammers. Together they were the plastics of the world before plastic.

Difficulty
●●●●●
Time
An afternoon for an awl or a toggle; a day for a spoon or a cup once the horn is prepared; horn cores take one to six weeks to loosen
Steps from zero
2 prerequisites →

You need first

Stone ToolsFire

This unlocks

Buttons, Buckles, Hooks and Zips
The full path from nothing — 2 steps before this one
  1. Stone Tools
  2. Fire
  3. Horn and Bone Working

Do them roughly in this order. See it on the tech tree →

Why it matters

Every animal you eat leaves behind horns and bones, and deer drop their antlers every winter. Worked, they become the small, tough things a household needs every day: spoons and cups that do not break when dropped, combs (Brooms, Brushes and Combs), buttons and toggles (Sewing, Needles and Thread), awls and needles, handles for knives and tools, and thin translucent panes to keep the wind off a candle (Lamps and Candles).

Horn behaves like a natural plastic: heat it and it goes soft; press it and it keeps its new shape when it cools. Until celluloid and the other Early Plastics arrived in the late 1800s, horn did most of the jobs plastic does now. Bone and antler are the hardest, stiffest materials you can get before metal.

How it works

Horn and bone are different materials, though they come from the same animal.

  • Horn is the hollow sheath on the heads of cattle, sheep, goats and buffalo. It is keratin — the protein of fingernails and hair — laid down in thin layers like pages rolled into a cone, around a core of living bone. Keratin softens at about the temperature of boiling water and stiffens again as it cools, keeping whatever shape it was held in. Much hotter (above about 200 °C) it blisters, browns and smells of burnt hair. Because it is layered, soaked horn can be split into thin leaves that let light through.
  • Bone is a hard mineral (calcium phosphate) held together by tough protein fibres (collagen). Heat does not soften it; it only makes it brittle. Bone is shaped by sawing, grooving, scraping and grinding. The dense walls of the long leg bones are the working material.
  • Antler is bone that deer, elk and moose grow and shed every year: a hard outer layer over a spongy core. It is tougher and springier than ordinary bone, so it makes hammers, picks and wedges. Soaking softens its surface and makes it much easier to cut.
sheath bony core cut off with a little skull 1 Remove the core soak 2–6 weeks, or boil 1–2 hours 2 Soften boiling water, 20–60 min, until it bends like leather horn between iron plates screw or wedge 3 Slit and press flat warm, greased plates; leave until cold thin leaf blunt knife 4 Split into leaves soak 2–4 weeks; scrape to 0.5 mm for lanterns
Fig. 1 Preparing horn. Soak or boil the horn until the bony core comes out; boil the empty sheath until it bends like leather; slit it and press it flat between warm, greased plates; for lantern panes, soak the flat plate and split it into thin leaves.

What you need

Item Notes
Cattle horns The best: big, hollow, fairly straight. Pale horns make the clearest panes. Sheep and goat horns are smaller and more solid — good for handles and buttons
Long bones Cannon bones (metapodials — the straight bones between knee or hock and hoof) of cattle, horses and deer; shin bones; ribs for flat pieces
Antler Shed antlers of red deer, elk, moose, reindeer or white-tailed deer
A big pot For boiling horn and simmering bone (Pottery)
Cutting tools Saw, knife, files and steel scraper (Files and Saws, Axes, Chisels, Knives and Planes); before metal, flint flakes and burins (Stone Tools)
A press Two smooth iron plates or flat hardwood boards about 20 × 30 cm, squeezed by wedges, a screw (Screws, Nuts and Bolts) or heavy stones
Drill A bow drill with flint or iron bits (Drills and Boring)
Abrasives and finish Sandstone slab, fine sand, powdered pumice, sifted wood ash or chalk, leather (Abrasives and Grinding Stones); tallow, oil or beeswax

Where to find it

  • Horns: from slaughtered cattle, sheep and goats (Butchery and Meat). Fresh horn is best; horns left out in the weather go grey, chalky and cracked on the outside. Saw the horn off with 2–3 cm of skull at its base so the core comes out whole.
  • Bones: ask for the lower legs, which carry almost no meat and are often thrown away. Bones that have lain outside for years are cracked and crumbly — use them only for practice.
  • Antler: shed in late winter and spring. Search feeding grounds, deer trails and woodland edges soon after; rodents gnaw old ones.

Warning Never take horn, bone or hide from an animal you find dead of unknown cause, especially one that died suddenly, did not stiffen, or has dark blood at the nose, mouth or anus. These are signs of anthrax, whose spores survive in horn, bone and hide for decades. See Dangers.

Preparing horn

  1. Get the core out. Soak the horns in water for 2–6 weeks until the core rots loose, then knock the horn mouth-down on a stump. It stinks: do it far from the house. Quicker: boil for 1–2 hours and knock the core out while hot (hold it in a thick cloth). See also Brooms, Brushes and Combs.
  2. Cut it up. The solid tip (the last 5–15 cm) is for handles, toggles and buttons. The hollow part is for sheet and spoons; a straight section from the wide end makes a cup.
  3. Scrape off the rough grey outer skin.

Softening. Boil the horn for 20 minutes (thin) to an hour (thick cattle horn), until a cut edge bends like stiff leather. For a tighter bend, hold it over glowing embers, never flames, turning constantly. Stop at once if it smokes, bubbles, browns or smells strongly of burnt hair — that horn is ruined. It stiffens within a minute or two of leaving the heat, so have the press or mould ready and work fast; if it stiffens, put it back in the water.

Pressing flat sheet.

  1. Slit the softened hollow horn down one side and prise it open with sticks or tongs.
  2. Grease the press plates thinly with tallow and warm them — hot enough that a drop of water spits on them (roughly 100–150 °C). Cold plates chill the horn before it flattens.
  3. Squeeze hard, tightening a little more every few minutes as the horn yields. Leave it under pressure until quite cold, an hour or more, or it slowly curls back.
  4. You now have a plate 2–4 mm thick. Store plates flat under a weight.

Lantern panes. Old lanterns were spelled lanthorn because their panes were horn.

  1. Soak flat plates in water for 2–4 weeks, or boil them for several hours, until the layers loosen at the edges.
  2. Work a thin, blunt knife into the edge and peel the plate into leaves 0.5–1 mm thick, while it is wet and warm. Good horn gives two to four leaves.
  3. Scrape each leaf from the middle outwards until it is about 0.5 mm thick and large writing shows through it.
  4. Press again between hot greased plates. Thin, smooth horn is amber and translucent: it passes a soft light but you cannot see clearly through it.
  5. Slide the leaves into slots in a wooden or tinned-iron lantern frame (Sheet Metal and Rolling). A horn lantern does not shatter when dropped and keeps a candle alight in wind and rain. The same thin horn protected the lesson sheet of a child's hornbook (Teaching and Schools).

Making things from horn

squeeze until cold, about 30 minutes Domedblock Hornsoftened Hollowblock trimmed andscraped Pressing a spoon hardwood mould, greased Horn tubewide end up,8–12 cm tallwall 2–3 mm Base discsprung in while hot groove 1 mm deep A horn cup the horn shrinks and grips
Fig. 2 Moulding horn. Softened horn is squeezed between a domed block and a hollow block until cold, then trimmed into a spoon. A horn cup is a straight section of horn with a flat horn disc sprung into a groove inside its narrow end.

A pressed spoon

  1. Carve a mould from two blocks of close-grained hardwood (beech, birch, maple) about 20 × 8 × 5 cm: one with a hollow shaped like a spoon bowl (about 6 × 4.5 cm, 1.5 cm deep), the other with a matching dome 3 mm smaller all round to leave room for the horn. Add a shallow channel for the handle. Grease both.
  2. Cut a blank from flat horn plate about 18–20 cm long, 6 cm wide at the bowl end and 2–2.5 cm at the handle end.
  3. Boil it for 30 minutes, lay it over the hollow, set the dome on top and squeeze — in a press, with wedges, or by standing on it — until cold, about 30 minutes.
  4. Trim with saw and knife, round the edges with a file, and scrape the bowl to an even 2–3 mm. Polish (below).

A horn spoon does not taint food and does not break. Highland Scots, among many others, ate with them for centuries.

A horn cup

  1. Saw a straight tube 8–12 cm long from the wide end of a big cattle horn. The narrow end will be the bottom.
  2. Boil it and push it, hot, over a tapered wooden former (a carved hardwood cone) to round it and even the wall. Let it cool there, then scrape the wall to 2–3 mm.
  3. Cut a groove round the inside, 6–10 mm from the narrow end and about 1 mm deep, with a knife point or small hooked scraper.
  4. Cut a base disc from 3 mm horn plate, 2–3 mm wider than the inside of the tube at the groove.
  5. Boil the tube 15 minutes, squeeze the narrow end oval, slip the disc in at an angle and spring it into the groove. As the horn cools and dries it shrinks and grips the base.
  6. Fill it with water. Seal any seep by rubbing beeswax into the joint from inside while the cup is warm.

Horn cups must not hold boiling liquids — heat softens and distorts them. Wash them in warm water.

Buttons, handles and other pieces

  • Buttons. Strike discs out of softened horn sheet 2–4 mm thick with a hollow punch — a short iron tube sharpened at one end (Blacksmithing) — on an end-grain block. Dome them by pressing while hot into a greased hollow. Drill two or four holes 1.5–2 mm across, from both sides.
  • Handles. Drill the solid tip of a horn with a hole a little smaller than the tool's tang (the spike behind the blade). Boil it 20 minutes and tap the tang in. Cooling horn clamps the tang; a little hot pitch or hide glue makes it permanent (Tar, Pitch and Glue, Glues and Adhesives).
  • Toggles, pegs, shoehorns, scoops and funnels are bent, pressed or cut the same way.
  • Horn waste — shavings and scraps — is rich in nitrogen. Dig it into the garden, where it rots slowly over a year (Compost and Manure).

Polishing

  1. Scrape away tool marks with a steel scraper, or a broken-glass edge held upright and pulled towards you.
  2. Rub with wet fine sand on leather, then powdered pumice and water.
  3. Finish with sifted wood ash or chalk and a drop of oil on leather or the palm of your hand until the surface goes glassy. Wipe with a trace of tallow.

Working bone

joint end knuckle blank,leveredout Groove and splinter cannon bone; cut both grooves right through the wall knuckle= handle point groundon sandstone 12–15cm Awl half a split cannon bone cord loop coat edge Toggle 4–6 cm, hole across the middle tooth centre slab 3–4 mm thick; holes left behind Button bit centre point and one cutting tooth
Fig. 3 Bone and antler. Grooves cut down a cannon bone let you lever out straight blanks. Split with the knuckle left on, it makes an awl. A toggle is a short tube with a hole across the middle; a button bit cuts round blanks out of a flat slab.

Preparing it

  1. Strip meat and tendons with a knife.
  2. Simmer, do not boil hard, for 1–3 hours, until the last flesh and the outer membrane scrape off. Long, hard boiling cooks the protein out and leaves bone chalky and brittle.
  3. Push out the marrow with a stick (eat it, or render it).
  4. Degrease in warm water with a handful of wood ash for a few days, changing the water when it clouds. Grease left in bone yellows and smells.
  5. Bleach on grass in the sun for 2–4 weeks.
  6. Work it fresh if you can: fresh bone is tougher and cuts more easily. Soak old, dry bone in water overnight first.

Cutting and shaping

  • Sawing: a fine metal saw cuts bone easily; keep it wet. Without a saw, score a ring round the bone with a flint edge, deepen it, and snap.
  • Groove and splinter: scratch two parallel grooves down a cannon bone with a flint burin or file until they cut right through the wall, then lever out the straight strip between them — the method for bone needles (Sewing, Needles and Thread).
  • Splitting: deepen the natural shallow groove down the front of a cannon bone, then tap a wedge into one end to split it lengthways.
  • Grinding on wet sandstone, turning constantly; bone grinds fast, so check often. Drilling with a bow drill, from both sides. Turning on a The Lathe for beads, pegs and handles.

Things to make

  • Awl — the most useful bone tool. Split a deer or sheep cannon bone lengthways, keeping the knuckle (the rounded joint) as a handle that fills the palm. Grind the shaft to a round, tapering point over the last 5–6 cm. A 12–15 cm awl punches holes in leather for sewing and opens knots and splices. Regrind it when it blunts.
  • Toggle — a tube of bone 4–6 cm long with a hole drilled across the middle or a groove round it. Tied to a cord and pushed through a loop, it closes a coat faster than a button and works with cold hands.
  • Handles — a section of hollow leg bone is already a handle: plug the marrow hole with a tight wooden plug and drive the tang into that. For a flat tang, rivet two flat bone scales either side (Nails, Rivets and Wire Fasteners).
  • Buttons — saw slabs 3–4 mm thick from a big cattle cannon bone or a shoulder blade, grind them flat, and cut discs with a button bit: an iron bit with a centre point and one cutting tooth set out at the radius you want, spun in a bow drill or brace. Cut halfway from each side and the disc drops out. Slabs riddled with round holes are found wherever bone buttons were made.
  • Spatulas and flat spoons — saw a cattle rib to length and split it edgeways into two thin plates.
  • Also needles (Sewing, Needles and Thread), fish hooks (Fishing), bird-bone whistles (Musical Instruments), pins, beads and weaving tools (Tablet and Band Weaving). Waste bone makes glue (Glues and Adhesives), fertiliser, and bone ash for Phosphorus and the cupels used to assay Gold and Silver.

Working antler

  1. Soak the antler in water for 1–3 days. The outer layer softens enough to cut perhaps twice as fast as dry antler. Keep it wet while working.
  2. Cut off tines (branches) and lengths of the beam (main stem) by sawing, or by grooving a ring and snapping.
  3. For straight blanks, groove and splinter as for bone; the grooves need only pass through the hard outer layer.
  4. Uses:
    • Hammers and pressure flakers for knapping flint (Stone Tools): a 20–30 cm piece of beam, or a tine. Antler strikes flint without shattering.
    • Handles: the spongy core of a tine is easy to drill out, and a tang driven in holds well.
    • Axe sleeves: a short, thick socket of antler that holds a small stone axe head and fits into a wooden haft, soaking up the shock that would split the haft.
    • Wedges for splitting logs, picks for digging chalk and hard ground, riveted combs (Brooms, Brushes and Combs), toggles and buttons.

How to tell it worked

  • Flat horn stays flat for weeks. A plate that slowly curls was released while still warm.
  • Lantern horn glows evenly when held up to the sun — no dark patches (too thick) or white crazing (scorched).
  • A horn cup holds water for a day without a drip; a spoon is evenly thin with no crack at the neck.
  • Good bone is creamy white, odourless, and rings faintly when tapped on stone.
  • An awl pushes through wet leather 3 mm thick by hand and survives a gentle twist.

Note Troubleshooting. Horn cracks when bent → not soft enough, or old weathered horn; boil longer or use fresher horn. Horn blisters or browns → too hot; use boiling water or embers only. Horn springs back → released too soon or plates were cold. Leaves will not split → soak longer; if the plate was pressed too hot its layers have fused — use it for buttons. Cup base leaks or falls out → groove too shallow or disc too small; cut deeper, make the disc 2–3 mm oversize, spring it in hot. Bone splits the wrong way → grooves not deep enough before levering. Bone smells and yellows → grease left inside; degrease again in warm ash water.

Dangers

Danger Anthrax. Its spores survive for decades in the hides, hair, horns and bones of animals that died of it, and in the soil where they lay. Handling such material causes black, painless sores; breathing its dust ("woolsorters' disease") often kills. Use only horn and bone from healthy animals killed for food, or shed antler. If someone who has handled raw animal material gets a painless sore with a black centre and swelling around it, seek medical help at once (Infectious Diseases).

  • Dust: sawing and grinding bone, horn and antler makes fine dust that irritates the lungs. Work wet, outdoors, with a damp cloth over nose and mouth.
  • Burns: boiling water, hot plates and hot horn all burn; handle softened horn with tongs or thick leather. If you soften horn in hot fat, never let it smoke, keep a lid ready, and never pour water on burning fat (Soap).
  • Splinters and cuts: bone splinters are needle-sharp and drive dirt deep. Cut and scrape away from your body and holding hand; clamp small pieces. Clean every cut at once (Wound Care and Antiseptics).
  • Smell and vermin: soaking horns and simmering bones stink and draw flies and rats. Do it far from the house and water supply, in covered tubs (Household Pests).

What this unlocks

Horn and bone give a household spoons, cups, buttons, combs, needles and handles at almost no cost. Bone glue joins Furniture and Musical Instruments; bone ash leads to Phosphorus; horn panes give Lamps and Candles their lanterns. When you reach Early Plastics you will find celluloid was invented to imitate horn, ivory and tortoiseshell — and every shape you learned to press in horn can be pressed in plastic.

How it was first done

Bone was one of the first materials people worked. Worn bone pieces from Swartkrans cave in South Africa, between about 1 and 1.8 million years old, were probably used by early humans to dig into termite mounds. Eyed bone needles appear by about 40,000 years ago in Siberia and then across Eurasia, making close-fitting layered clothes possible in the Ice Age. About 4,500 years ago, miners at Grimes Graves in England dug shafts to the flint with hundreds of red-deer antler picks.

Horn was worked wherever cattle were kept. Around 893, Asser, the biographer of Alfred the Great, wrote that the king had lanterns made of wood and thin horn so that the candles he used to measure time would not gutter in the draughts. From the 1400s to the 1700s children learned their letters from hornbooks. Horners had guilds in medieval cities; the London Horners' Company received a royal charter in 1638. Horn buttons, combs, spoons and lantern panes were made in huge numbers until celluloid and then modern plastics took over in the late 1800s and 1900s.

Source: content/entries/home/horn-and-bone-working.md