◆ Rebuild

Part 7 · Home and Daily Life

Wood Turning and Treen

The turner's craft beyond the first tool handle — forging and grinding gouges, skews, parting tools, scrapers and hook tools; building a treadle lathe with a faceplate; and turning treen — bowls, platters, spoons, handles, chair legs, spindles and lidded boxes — and finishing them safely for food.

Difficulty
●●●●●
Time
A day to forge a set of tools; an hour for a chair leg; a day for a bowl, spread over two months of drying
Steps from zero
16 prerequisites →

You need first

The LatheAxes, Chisels, Knives and Planes

This unlocks

—
The full path from nothing — 16 steps before this one
  1. Stone Tools
  2. Cordage and Rope
  3. Fire
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Basic Woodworking
  7. Hunting and Trapping
  8. Charcoal
  9. Hides and Leather
  10. The Wheel and Axle
  11. Bellows
  12. The Lathe
  13. Iron (the Bloomery)
  14. Blacksmithing
  15. Steel
  16. Axes, Chisels, Knives and Planes
  17. Wood Turning and Treen

Do them roughly in this order. See it on the tech tree →

Why it matters

Treen — "made of tree" — is the old word for the small wooden things of a household: bowls, plates, spoons, boxes, rolling pins, tool handles, chair legs and rungs, spinning spindles, pegs and knobs. Before cheap pottery and metal, most families ate every meal from turned wooden bowls, and they are still among the best: light, unbreakable, quiet, warm to hold, and made from a log in a day.

The The Lathe chapter shows how to build a pole lathe and turn a first tool handle. This chapter is the craft that follows: a full set of turning tools, a lathe that turns continuously, and how to make each kind of treen well enough to sell. The same cuts make parts for Furniture, spinning wheels, Toys, Musical Instruments and pulleys.

How it works

Cut, don't scrape. A sharp tool held with its bevel rubbing the wood slices off a shaving like a plane and leaves a shiny surface. A tool held flat, edge first, scrapes off dust and tears the fibres. Scraping is safer for beginners and useful for awkward hollows; cutting is faster and cleaner.

Cut downhill. Wood fibres are like a bundle of straws; cut so each is supported by the ones beneath it.

  • Spindles (grain along the lathe): cut from a larger diameter towards a smaller one — down the sides of a bead, into the bottom of a cove.
  • Bowls (grain across the lathe): outside, from the foot towards the rim; inside, from the rim towards the centre. The wrong way tears the end grain in two patches opposite each other.

Green and dry. Green wood cuts easily but shrinks as it dries, more across the growth rings than along them, so a round bowl goes oval and a box lid stops fitting. Turn green for chair parts, rough bowls and anything that may move; turn dry for boxes and platters.

Speed. On a continuous lathe, a safe starting speed is about 15,000 ÷ diameter in cm turns a minute, but no more than about 2,000 even for thin work: a 5 cm spindle at 1,500–2,000, a 25 cm bowl at 600, a 40 cm platter at 350–400. Rough or unbalanced work goes slower. A pole lathe never goes too fast.

What you need

Tool Made from Width Bevel Use
Roughing gouge Flat bar 6 mm, forged to a deep U 20–30 mm 45°, square across Billet to round
Spindle gouge Flat bar 5 mm, a shallow U 10–13 mm 30–35°, rounded nose Beads, coves, detail
Bowl gouge Flat bar 8 mm, deep U, thick walls 10–16 mm 45–55° Bowls inside and out
Skew chisel Flat bar 6 × 22 mm 20–25 mm 20–25° each face; edge slanted 20–30° Planing cuts, beads
Parting tool Bar 4–6 × 15 mm 3–6 mm 25° each side to a point Sizing cuts, cutting off
Scraper Bar 6–10 mm thick 20–30 mm 70–80°, with a burr Smoothing hollows
Hook tools Round bar 10–12 mm, end flattened and bent Hook 2–4 cm 30°, inside Hollowing on a pole lathe

Also: the pole lathe from The Lathe or a treadle lathe (below); wooden calipers and dividers; a grindstone and slipstones (Sharpening and Honing); axe and saw for blanks; hide glue and paper (Glues and Adhesives); oil and beeswax. Handles are ash or beech, 30–40 cm for spindle tools and 45–60 cm for bowl and hook tools, with a ferrule of iron or copper tube (Metal Pipes and Tubes) so the tang does not split them.

Where to find it

  • Bowl wood. Fresh logs 25–45 cm across of birch, beech, sycamore and maple, alder, cherry and other fruitwoods, lime, ash, poplar or willow — straight, unknotted, sound. Use within weeks, or keep the logs whole with the ends sealed with wax or clay.
  • Box wood. Dense, fine, very dry wood: box, hawthorn, apple, pear, plum, holly, maple, olive. Branches 6–10 cm thick, split through the pith, dried a year in a dry room.
  • Spindle wood. Ash, beech, oak, maple, hickory, split (not sawn) so the billet follows the grain.
  • Finishes. Linseed and walnut oil (Oils and Pressing), beeswax (Beekeeping), lac for shellac (tropical), horsetail stems from wet ditches.

The tools

TURNING TOOLS side view end side view end 45° 30–35° 45–55° toe heel (from above) 25° each side 70–80° burr Roughing gouge deep U, square end billet to round Spindle gouge shallow U, nose rounded beads and coves Bowl gouge deep U, thick walls handle 45–60 cm Skew chisel edge slanted 20–30° 20–25° bevel each face Parting tool bevels meet at a point; wider at the edge Scraper steep bevel, burr on top; handle above the edge Hook tool flat end bent to a hook, honed inside, about 30° All of them 0.8–1 % carbon steel, tempered dark straw to brown (240–260 °C); handles 30–60 cm of ash or beech with a ferrule
Fig. 1 Turning tools seen from the side, with the end view of each blade and its bevel angle. Gouges are forged U-shaped from flat bar; the skew and parting tool are flat; the scraper works with a burr; the hook tool hollows bowls on a pole lathe.

All turning tools are high-carbon Steel (0.8–1 % carbon), forged at an orange heat (Blacksmithing), hardened by quenching from dull cherry red (where a magnet stops sticking, about 780–800 °C), and tempered a little softer than bench chisels because they take hard knocks: dark straw to brown, 240–260 °C. Old files make fine tools, but soften them to blue first; a glass-hard file scraper can shatter on a catch.

Roughing gouge

The workhorse for taking a billet down to round. Forge a bar 6 mm thick, 30 mm wide, 25 cm long, and draw a 10 cm tang. At orange heat, lay the blade over a U-shaped groove in a swage block and drive a round bar about 18 mm thick down into it, working from tang to tip, until it is a deep U. Grind the end square across at 45°. A good one has even walls and an edge that touches the wood along its whole curve.

Spindle and bowl gouges

The spindle gouge is shallower and lighter (bar 5 mm × 13 mm), its nose ground round like a fingernail with the sides swept back, at 30–35°; it cuts beads, coves and detail. The bowl gouge is forged deep and thick-walled from 8 mm bar so it can reach 10 cm over the rest into a bowl without chattering; grind it at 45–55° (steeper for deep bowls) and fit a long handle. Roll a gouge as you grind so the bevel follows the curve.

Skew chisel

A flat chisel bevelled on both faces, its edge slanted across; the long corner is the toe, the short one the heel. It gives the cleanest finish of any tool — a planing cut that leaves the wood shining — and catches hardest when misused. Grind each face to 20–25° and slant the edge 20–30° from square. Cut only with the lower half of the edge, near the heel; if the toe touches the spinning wood, it digs in.

Parting tool

A narrow tool with two bevels meeting at a point, pushed straight in to cut a groove to depth or to cut work off. File its sides so it is slightly wider at the edge than behind, or it binds and burns in its own groove.

Scraper

A thick bar ground at 70–80° and held pointing slightly downhill (handle higher than the edge) so it cannot dig in. Raise a burr by stroking the top face along the edge with a hardened, polished steel rod. The burr cuts fine curls inside boxes and bowls.

Hook tools

The pole-lathe bowl turner's tools. Flatten the last 6 cm of round bar 10–12 mm thick to about 3 mm, bend it into a hook — gentle for walls, tight for the bottom — and hone the inside at about 30°. Fit handles 60 cm long, held under the arm and levered over a pin in the rest. Three to five hooks of different curves do all the hollowing.

Keeping them sharp

Grind on a wet grindstone (Abrasives and Grinding Stones) with the bevel flat on the stone, rolling gouges so the whole curve meets it. Take the burr off the inside of gouges with a round slipstone. A turner touches up every 10–20 minutes of cutting. See Sharpening and Honing.

The treadle lathe

A pole lathe cuts only on the down-stroke. A treadle lathe turns one way all the time, and with a faceplate it holds work from one end only — the key to boxes, platters and bowls you can see into.

  1. Flywheel and crank. Under the bed, mount a flywheel 60–90 cm across and 25–40 kg on a cranked iron axle with a throw of 8–10 cm; a rod joins the crank to a treadle (Cranks, Cams and Linkages).
  2. Headstock. A heavy block on the left of the bed carries an iron spindle 2.5–3 cm thick in two bronze or hardwood bearings (Bearings and Lubrication), with a collar for end thrust and a small pulley 5–8 cm across, stepped if you can.
  3. Belt. A round or flat leather belt (Belts, Chains and Power Transmission) from flywheel to pulley. A 75 cm flywheel driving a 6 cm pulley, trodden 60–80 times a minute, spins the work at 700–1,000 turns a minute — right for spindles. Use the largest pulley step for bowls.
  4. Spur drive. For spindles, a centre point between two chisel-shaped prongs that bite into the end of the billet; the other end runs on a greased tailstock centre.
  5. Faceplate. An iron disc 10–15 cm across, threaded or keyed onto the spindle nose, with four to six countersunk holes. Screw the bowl or platter blank to it with screws 2.5–3 cm long into wood that will be cut away. A hardwood disc on a threaded wooden boss serves for light work.
  6. Chucks. A jam chuck is scrap wood on the faceplate with a recess or spigot turned to grip the work by friction — for holding a bowl or box upside down to finish the base. A glue chuck: glue the work to a waste block with hide glue and a sheet of paper in the joint; a chisel tapped into the paper later splits them cleanly.

A belt from a The Watermill or line shaft can drive the same headstock (Planers, Thicknessers and Woodworking Machines); the dangers below then apply with full force.

Treen, step by step

Spindles and rungs

A spindle is any long turned rod with the grain along it: chair rungs, balusters, rolling pins, pegs, drop spindles for spinning, bobbins. To make many alike:

  1. Draw the full-size profile on a strip of wood — a story stick — with a mark at each change of diameter.
  2. Rough the billet round, hold the stick against it, and pencil the marks onto the spinning work.
  3. At each mark, cut down with the parting tool while holding calipers set to that diameter in the groove, until they slip over. These sizing cuts fix every diameter.
  4. Join them with gouge and skew: beads rolled down from their tops, coves cut from both rims to the bottom.
  5. Support long thin work (under 2.5 cm thick, over 30 cm long) with your fingers lightly behind the cut, or a notched steady clamped to the bed.

A chair rung is typically 30–45 cm long, 2.2–2.5 cm thick in the middle, with tenons 16 mm across and 2.5–3 cm long.

Chair legs

Turn a leg like a spindle from a green split billet 5 × 5 × 45–50 cm, to 3.5–4.5 cm at its thickest, with a 22–25 mm tenon at the top if it goes through a seat (Furniture). The chairmaker's trick makes joints that never loosen:

  1. Turn the rungs green, then dry them hard for a week or two near a stove.
  2. Turn their tenons again, a hair oversize for the holes.
  3. Turn the legs green and bore the rung holes while they are still damp.
  4. Drive the dry rungs into the damp legs. The legs shrink onto the tenons while the rungs swell slightly. The joint locks without glue.

A good set of legs is straight when rolled on a bench and matches bead for bead within 1 mm.

Tool handles

Turn as in The Lathe, leaving a short cylinder at the front the exact inside size of a ferrule cut 1.5–2 cm long from iron or copper tube. Tap the ferrule on, bore the tang hole slightly undersize, and drive the tool in. Chisel and file handles are 10–14 cm long.

Bowls

The central piece of treen, and the hardest to do well.

1 The blank half a log; rim towards the pith bowl inside the half log pith zone: cut away 2 Rough-turn, then dry walls a tenth of the width; 6–12 weeks in its shavings paper sack 2.5 cm wall 3 Finish-turn walls 5–7 mm, base 8–10 mm; cut downhill on the grain outside: foot → rim inside: rim → centre even wall
Fig. 2 Turning a bowl. Split a log through the pith and keep the pith out of the blank. Rough-turn it green with walls a tenth of its width, dry it slowly in its own shavings, then turn it again to its final thin, even wall.
  1. Blank. Split a green log in half through the pith. The pith and the 2–3 cm beside it always crack: cut them away. Scribe a circle on the flat face and saw or chop it round. A blank 25 cm across and 12 cm thick makes a serving bowl.
  2. Mount it.
    • Pole lathe: drive a mandrel — a hardwood cylinder 6–8 cm across and 20 cm long with three iron spikes in one end — into the centre of the base, and wrap the cord round it. Turn the outside, then hollow with hook tools, leaving a cone-shaped core round the other centre. Knock the core off when the walls are done and carve away the stub.
    • Treadle lathe: screw the faceplate to the rim face, turn the outside and a foot or small recess to grip later, then reverse the bowl onto a jam chuck and hollow it.
  3. Once or twice turned.
    • Once-turned: turn the green bowl straight to an even 6–8 mm wall. It dries in a week or two without cracking but warps oval, as most old treen bowls are.
    • Twice-turned: rough it green with walls a tenth of the diameter (2.5 cm for a 25 cm bowl). Dry it in a paper sack of its own shavings in a cool, shady place for 6–12 weeks, weighing it weekly until the weight stops falling. Then turn it round again to 5–7 mm walls. It stays round.
  4. Shape the inside to follow the outside so the wall is even all the way down; feel it between finger and thumb. Leave the base 8–10 mm thick over a foot ring.
  5. Cut downhill, and take a last fine cut with a freshly honed gouge.

Sizes: a porridge bowl 15–16 cm across and 6–7 cm deep; a serving bowl 25–30 cm; a dough bowl 40–50 cm. A good bowl is light for its size, has no torn patches, sits flat, and has no cracks running in from the rim. A crack along the pith line means the pith was left in.

Platters

A platter is a wide, shallow plate 30–40 cm across, from dry flat board 2.5–3 cm thick (Sawmills and Lumber, or split and planed). Green platters warp too much to use. Screw the faceplate to the top face, turn the underside flat with a low foot ring, reverse onto a jam or glue chuck, and turn the top with a flat centre and a broad rim, leaving it 1.2–1.5 cm thick. Check it with a straight stick across it while stopped.

Lidded boxes

LIDDED BOX (SECTION) HOLLOWING THE BASE grain runs along the axis Lid recess 5–6 mm deep Spigot cut a whisker at a time until the lid pops on Walls 3–4 mm Floor 5–6 mm Jam chuck grips the tenon Box base end grain Spindle gouge cut from the centre outward
Fig. 3 A lidded box in section. Both parts are turned from one dry end-grain blank. The lid's recess fits over a spigot on the base; the base is held in a jam chuck to hollow it.

A small round box whose lid fits with a soft pop is the test of a turner. Use dry, dense end-grain wood.

  1. Turn a blank 6–8 cm square and 12 cm long to a cylinder between centres, with a short tenon at each end.
  2. Part it into lid (about a third) and base (two thirds).
  3. Lid: held in a jam chuck by its tenon, hollow it and cut a recess 5–6 mm deep with a dead-straight wall.
  4. Base: held by its tenon, cut a spigot at the rim 5–6 mm long, slightly too big. Hollow the inside with the spindle gouge, cutting from the centre outward, and smooth with a scraper to walls 3–4 mm thick.
  5. Fit: shave the spigot a whisker at a time, trying the lid after each cut, until it goes on with firm hand pressure. One cut too many and it rattles.
  6. With the lid on, turn the outside of both together so the outline and grain run straight through; then finish top and bottom on jam chucks.

Spoons

A spoon is mostly carving (Cutlery and Tableware), but the lathe gives a round handle and bowl back. Turn the whole spoon as one spindle 20–25 cm long: a ball 5–6 cm across at one end and a handle 1.2–1.5 cm thick. Saw away the top third of the ball down to the line of the handle and hollow the bowl with a hook knife. A ladle is the same, larger.

Finishing

  1. Burnish by pressing a handful of the work's own shavings hard against it as it spins.
  2. Smooth if you must with sand glued to cloth (Abrasives and Grinding Stones), coarse to fine, at slow speed, keeping it moving; finish with a bundle of dry horsetail. Clean tool work needs little sanding.
  3. Oil for food. Wipe on thin coats of raw linseed or walnut oil — oils that dry hard in air — and wipe off all surplus after 15 minutes; three to five coats a day apart. Cooking oils like olive or sunflower never dry and can go rancid. Many working bowls are best left bare and scrubbed.
  4. Oil and wax. Melt 1 part beeswax into 4 parts oil in a pot standing in hot water, and rub it onto the spinning work with a cloth until it warms and shines — for handles, spindles and boxes.
  5. Shellac friction polish. Dissolve 1 part lac flakes in 5 parts strong alcohol (Distillation); hold a cloth pad charged with it and a drop of linseed oil on the spinning work. It gives a bright gloss in minutes, but hot drinks and alcohol mark it: for boxes and knobs, not bowls or cups.

How to tell it worked

  • Surface straight from the tool shines, with fine even spiral marks; fuzzy, torn patches show an uphill cut or a dull edge.
  • Size: calipers slip over every bead and tenon with the same feel; four legs side by side line up.
  • Bowls and boxes: even walls; no cracks after drying; a lid snug all round.

Note Troubleshooting. Catches: the tool digs in and is torn down → bevel not rubbing, rest too low or far, or the skew's toe touching. Start every cut bevel-first, then raise the handle slowly. Rippled surface (chatter) → tool overhanging the rest, thin flexing work, or a loose faceplate. Torn end grain in two patches → cutting uphill or a dull tool; reverse the cut, sharpen, take a light last cut. Bowl cracks while drying → pith left in, dried too fast, or walls uneven. Box lid loose a month later → wood not dry; rough-turn boxes and let them settle a few weeks before fitting. Burn rings → sanding too hard or a dull parting tool.

Dangers

Danger Work can fly off the lathe. A blank with a hidden crack, a loose faceplate screw or too much speed can throw several kilograms of wood like a stone from a sling. Check blanks for cracks, use enough screws in sound wood, start slow, stand out of line of the work when starting, and protect your eyes.

  • Oily rags catch fire by themselves. Rags with linseed, walnut oil or oil-and-wax heat up as the oil dries and can burst into flame hours later in a heap. Spread them flat outdoors to dry, or keep them under water in a closed tin.
  • Dust. Yew is toxic; many woods cause rashes and asthma. Sand little, and cover nose and mouth when you do.
  • Powered lathes do not stop when you are caught: no loose sleeves, scarves, long hair or rags, and a way to stop the drive at once.
  • Long tools whip when they catch: both hands on them, fingers never between rest and work.

What this unlocks

A treen workshop supplies a village with bowls, plates, spoons and boxes for almost nothing, and the parts of Furniture, ladders, spinning wheels, looms (The Loom), Toys and Musical Instruments. Turned wooden patterns make castings (Metal Casting), and the hand control and tool geometry learned here carry over to turning metal on Machine Tools and to the The Potter's Wheel.

How it was first done

Turned wooden bowls were common in Europe by Roman times. At Coppergate in York, Viking-age turners of the 10th century left thousands of the cores knocked from the middles of pole-lathe bowls — the method in this chapter. Medieval treen was everyday tableware, and mazers, maple drinking bowls with silver rims, were left in wills. Pole-lathe bowl turning lasted in England until George Lailey of Bucklebury, the last traditional bowl turner, died in 1958; it has since been revived from his tools. The treadle and flywheel lathe spread from the 16th century, and in the 19th the Holtzapffel family of London built ornamental lathes and wrote the great handbook of turning. Factories then turned chair legs and handles by the million on copying lathes that follow a template — a story stick made of iron.

Source: content/entries/home/wood-turning.md