◆ Rebuild

Part 15 · Knowledge and Science

Mirrors

How to make a mirror — polished bronze and the white, glassy speculum metal of the first reflecting telescopes, the old poisonous tin-and-mercury mirror, and the modern way, a film of pure silver laid on clean glass from a solution of silver nitrate — and how curved mirrors gather light for telescopes, lamps and solar furnaces.

Difficulty
●●●●●
Time
A day to cast and a week to grind and polish a metal mirror; an hour to silver a glass, once you have the chemicals
Steps from zero
23 prerequisites →

You need first

GlassSilver Nitrate and Silver Salts

This unlocks

Cooking Ranges, Iceboxes and Vacuum FlasksSignal Fires, Flags, Semaphore and HeliographsThe TelescopeVacuum Coating and Thin Films
The full path from nothing — 23 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. The Kiln
  10. Pottery
  11. Charcoal
  12. Hides and Leather
  13. Lime
  14. Lye and Potash
  15. Glass
  16. Bellows
  17. Saltpeter
  18. Copper Smelting
  19. Lead
  20. Sulfuric Acid
  21. Gold and Silver
  22. Nitric Acid
  23. Silver Nitrate and Silver Salts
  24. Mirrors

Do them roughly in this order. See it on the tech tree →

Why it matters

A mirror is more than a way to see your own face, though that matters too — for shaving, for dressing wounds you cannot otherwise see, and for doctors and dentists looking into mouths, ears and throats (Dentistry, Examining a Patient).

  • Light where it is needed. A mirror behind a lamp doubles the light on a workbench or a page (Lamps and Candles). A mirror at a window throws daylight into a dark workshop, a mine entrance or a sick-room. A small mirror under a The Microscope lights the specimen.
  • Signals. A flat mirror flashing sunlight can be seen 30–50 km away on a clear day — a heliograph sends messages in code over mountains without wires (The Telegraph).
  • Concentrated sunlight. A curved mirror brings the sun's light to a point: cooking, boiling water, melting metal and testing materials at furnace heat with no fuel (Solar Heat).
  • Telescopes. A curved mirror does the work of a lens without the coloured fringes that spoil simple lenses. The great telescopes are all mirrors (The Telescope).
  • Instruments. The sextant (Navigation), the mirror galvanometer (Measuring Electricity), the periscope, the camera (Photography).

How it works

Reflection. Light bouncing off a smooth surface leaves at the same angle at which it arrived, measured from a line square to the surface. A flat mirror therefore shows an image that seems to stand as far behind the mirror as the object stands in front of it.

Flat mirrorConcave mirror angle in angle out line square to the mirror The two angles are always equal glass in front, silver behind (a looking glass) F C parallel light from the sun or a star f = R ÷ 2 radius R C: centre of the sphere the mirror is part of F: the focus, halfway from C to the mirror
Fig. 1 How mirrors reflect. On a flat mirror, light leaves at the same angle as it arrives. A concave mirror turns parallel light from the sun or a star towards one point, the focus, which lies halfway between the mirror and its centre of curvature.

What makes a good mirror is a surface that is:

  1. Smooth — scratches and pits smaller than about a thousandth of a millimetre. Anything rougher scatters light and gives a grey, dull image. This is why mirrors must be polished, not just ground.
  2. Of a metal that reflects strongly. Fresh silver reflects about 95 % of the light that falls on it — more than any other material you can make. Polished speculum metal reflects about 60–65 %, bronze and copper somewhat less (and tint the image yellow or red). Polished obsidian or black glass reflects only 5–10 %, enough to see your face in daylight.
  3. The right shape. Flat for looking glasses and signals; curved for gathering light.

Curved mirrors. A concave mirror (hollow, like the inside of a spoon) gathers light. A spherical concave mirror of radius R brings sunlight to a focus at a distance f = R ÷ 2 from the mirror — half its radius. (Compare a lens, where f is about R.) A convex mirror (bulging) spreads light and shows a small, wide view — useful at blind corners.

For a perfect point focus the curve should be a parabola, not part of a sphere. But for mirrors that are shallow — the focal length at least 8 times the width — the difference is tiny, and a sphere, which grinding makes naturally (Lenses), is good enough.

Front or back. A glass mirror can be coated on the back (the light passes through the glass twice, which protects the silver; normal looking glasses) or on the front (the light never enters the glass; needed for telescopes, so the image is not doubled or coloured by the glass).

What you need

For Item Details
Metal mirrors Copper Smelting and tin (Tin and Pewter) 2 parts copper to 1 part tin by weight for speculum; 3 to 1 for a bronze mirror
Crucible, furnace, mould As in Metal Casting
Abrasives Sand, emery and rouge in graded sizes (Abrasives and Grinding Stones, Lenses)
Pitch Pine pitch for the polishing lap (Tar, Pitch and Glue)
Silvered glass Flat or ground Glass Clear, free of bubbles where the image matters; Window Glass for household mirrors
Silver nitrate From pure silver and Nitric Acid (Silver Nitrate and Silver Salts)
Ammonia water Strong, 15–25 %, from Ammonia
Caustic potash Potassium hydroxide, from Lye and Potash
A reducing sugar Cane or beet sugar boiled with a trace of nitric acid, or honey (Sugar, Beekeeping)
Distilled water Litres of it (Distillation); clean rainwater will do if you have no still
Glass or glazed dishes Shallow, a little bigger than the mirror. No metal
Chalk, soap, cotton For cleaning

Where to find it

  • Copper and tin ores: green malachite and copper minerals (Copper Smelting, Finding and Identifying Ores); heavy brown-black cassiterite pebbles in streams (Tin and Pewter).
  • Silver: native silver, or silver from lead ores (Gold and Silver, Lead).
  • Chalk: soft white limestone; a paste of fine chalk and water scrubs glass clean without scratching (Lime).
  • Honey: from wild or kept bees (Beekeeping). Its sugars are of the "reducing" kind that turn silver salts into silver metal.

Method 1: Polished metal mirrors

Simple and quick

A sheet of Copper Smelting, brass, silver or tinned iron, hammered flat, ground on a flat stone with fine wet sand, and polished with rouge on leather, makes a fair mirror in a day. Copper and brass give a warm, slightly coloured image; silver the best of all, but it tarnishes black in a few weeks (sulfur in the air) and must be repolished with chalk.

Speculum metal

Speculum is bronze with so much tin — about a third — that it is no longer golden but silver-white, hard and brittle as glass. It takes a brilliant polish and keeps it for months. It made the mirrors of the first reflecting telescopes.

  1. Weigh 2 parts of copper to 1 part of tin (for example 600 g and 300 g). A good fracture tells you the mix is right (step 6).
  2. Melt the copper in a crucible under a layer of charcoal, as for Bronze. When it is fully liquid, push in the tin, warmed first, in small pieces. Stir once with a dry green stick. The alloy melts much lower than copper; pour as soon as it is fully fluid.
  3. The mould. Make an open mould of fine, dry moulding sand or fired clay with a flat floor (Metal Casting), a little larger and 1.5–2 times thicker than the finished mirror needs — a 10 cm mirror should be cast about 1.5 cm thick. For a concave mirror, make the floor gently domed, so less grinding is needed. Cast face down: the bottom face, which cooled against the mould, is the one free of slag and bubbles.
  4. Cool very slowly. Speculum cracks from the slightest strain. As soon as it has set, cover the mould with hot ashes and charcoal, and let it cool over one or two days.
  5. Grind and polish. Grind the face flat (on a flat stone) or concave (on a convex tool), through grades of emery to the finest, exactly as for a lens (Lenses). Polish on a pitch lap with rouge or tin oxide ("putty powder"), with light pressure, for several hours. Speculum is hard; it grinds slowly.
  6. Check the metal. If a broken scrap shows a fine-grained, silvery-white face like steel, the alloy is right. A pinkish or yellow tinge means too little tin — softer and quick to tarnish. Coarse, glittering, bluish crystals that crumble mean too much tin.

Tip Speculum shatters if dropped or if its edge is struck. Grind a small bevel all round the edge before working the face, handle it over a padded bench, and never heat or cool it suddenly.

Method 2: The tin-and-mercury mirror (history only)

From the 1500s to the 1800s, the famous Venetian looking glasses were made by laying tin foil on a flat stone table, flooding it with mercury to make a soft silvery paste (an amalgam), sliding clean glass over it and weighting it for days while the extra mercury drained away. The mirror makers breathed mercury vapour all their working lives and suffered tremors, rotted teeth and madness (Mercury). Old mirrors made this way still drip droplets of mercury when they break.

Do not make these. Silver gives a brighter mirror, and the method below is far safer.

Method 3: Silvering glass with silver nitrate

1 Clean 2 Mix 3 Pour and rock 4 Rinse and protect Clean: water sheets in one unbroken film Greasy: water beads clean again soap, then chalk paste, then nitric acid on cotton, then distilled water. Never touch the face ammonia, drop by drop silver nitrate in water: brown cloud, then just clear; add potash, clear again; a few drops of silver to leave it faintly cloudy + reducer, pour at once rock gently brown → black; bright silver forms in 3–6 minutes at 20 °C Leftovers into salty water. Never store the mixture. you look in through the glass Looking glass: glass silver shellac or varnish oil paint Telescope mirror: silver on the front face; when dry, polish lightly with chamois and rouge; keep covered; resilver when it tarnishes
Fig. 2 Silvering glass. Clean the glass until water sheets off it. Make the silver solution with ammonia and potash, add the sugar reducer, pour it over the glass at once, rock it for a few minutes while the silver forms, then rinse and dry.

This is the chemistry of every mirror made from the 1850s until vacuum coating came in the 1930s, and of telescope mirrors made by amateurs ever since. It lays a film of pure silver, thinner than a thousandth of a millimetre, on glass.

1. Make the reducer (a week or more ahead)

Dissolve 10 g of cane or beet sugar in 100 ml of distilled water, add 0.5 ml (10 drops) of strong nitric acid, and boil gently for 5 minutes. This breaks the sugar into the "reducing" sugars that turn silver salts into metal. Let it cool and add 20 ml of strong alcohol to keep it. It improves with age and keeps for months in a stoppered bottle. (A teaspoon of honey dissolved in 100 ml of distilled water also works, and needs no acid or boiling; make it fresh.)

2. Clean the glass perfectly

Silver will not stick to glass that has the faintest film of grease.

  1. Scrub with soap and water, then with a paste of fine chalk and water on a pad of clean cotton.
  2. Rinse thoroughly, then swab the face with strong nitric acid on a wad of cotton tied to a glass rod, for a minute.
  3. Rinse with plenty of water, then with distilled water.
  4. Test: water should spread over the whole face in an unbroken sheet. If it pulls back into drops anywhere, clean again.
  5. From now on, never touch the face, and keep it under distilled water until the solution is ready.

3. Make the silvering solution (just before use)

For a mirror up to about 15 cm across:

  1. Dissolve 4 g of silver nitrate in 60 ml of distilled water in a glass jar. Pour off and keep back about a tenth of it in a separate cup.
  2. Add strong ammonia water drop by drop, stirring with a glass rod. A dark brown cloud forms. Keep adding drops until it just clears. Stop at once.
  3. Dissolve 2 g of caustic potash in 60 ml of distilled water and stir it in. The liquid turns dark brown-black again.
  4. Add ammonia again, a drop at a time, stirring, until it just clears once more.
  5. Now add a few drops of the silver solution you kept back, until the liquid stays faintly cloudy, pale straw-coloured. This ensures there is no spare ammonia, which would slow the silvering and spoil it.
  6. Strain it through a plug of clean cotton in a glass funnel.

4. Silver it

  1. Lay the glass, clean face up, in a shallow glass or glazed dish. (For a front-surface telescope mirror, many workers hang it face down in the solution, so dust and specks settle away from it.)
  2. Stir about 15 ml of the reducer into the silver solution and at once pour it over the glass.
  3. Rock the dish gently and steadily. Within a minute the liquid turns brown, then black, and a bright film appears on the glass. At about 20 °C it is complete in 3–6 minutes, when the liquid turns muddy grey with floating flakes. Colder, it takes longer; very warm, it goes too fast and gives a loose, dull coat.
  4. Pour off the spent liquid into a bucket of salted, vinegared water (see Dangers). Rinse the mirror gently with distilled water, then stand it on edge to dry.
  5. For a thicker, more opaque coat, clean the dish and repeat with fresh solution. Two coats are usual for a back-silvered looking glass.

5. Finish

  • A back-silvered looking glass: when dry, protect the silver with two coats of shellac or varnish, then a coat of oil paint. Light reaches it through the glass, and the silver never sees air.
  • A front-surface mirror (telescope, instrument): when completely dry, polish it very lightly with a pad of the softest chamois leather or cotton dusted with the finest rouge, using circular strokes and no pressure. It goes from slightly milky to brilliant. Keep it covered when not in use. Expect to resilver every few months to a couple of years, as sulfur in the air tarnishes it.

Curved mirrors

  • For a telescope, grind a concave glass or speculum mirror on a convex tool, exactly as for a lens, then polish and test it — the whole process is in The Telescope. The depth of the hollow at the centre is D² ÷ (16 × f) for a mirror D across with focal length f: a 15 cm mirror of focal length 120 cm is only 1.2 mm deep.
  • For cooking and solar furnaces, a large dish formed in clay or plaster to a parabola and faced with many small flat mirrors works well; see Solar Heat for the template. Each small mirror only needs to be flat; the dish gives the shape. A dish 1.5 m across concentrates enough sunlight to melt lead, zinc and aluminium at its focus.
  • For lamps, a concave reflector with the flame at its focus sends a strong parallel beam: a searchlight, a lighthouse, a miner's lamp.
  • A shaving or dental mirror is a gentle concave mirror with a focal length of 30–60 cm: it shows a face enlarged and upright when held closer than its focus.

How to tell it worked

  • Flatness. Hold the mirror so you see a long straight edge — a roof ridge, a taut string — reflected at a low angle. A flat mirror shows it straight; a wavy one bends it. Two good flat mirrors facing each other make a long, straight "tunnel" of reflections.
  • Silver coat. Hold the fresh silvered glass up to a bright light. A good coat is opaque, or shows only a faint blue glow. Pinholes appear as bright stars; a thin coat looks brown or blue all over.
  • Adhesion. Silver that peels or rubs off with a fingertip was laid on dirty glass.
  • Focal length. Turn a concave mirror to the sun and find the smallest bright spot on a card held in front of it; that distance is f (shade your eyes).
  • Brightness. Compare two mirrors side by side reflecting the same white wall. Good silver looks nearly as bright as the wall itself; speculum noticeably darker and slightly yellow.

Note Troubleshooting. Silver patchy, streaky or does not form on part of the glass → grease. Clean again with nitric acid; test that water sheets. Coat dull and powdery, rubs off as grey dust → the solution was too warm or too strong, or there was too much reducer. Use cooler solution, rock steadily. Nothing happens for many minutes → too much ammonia (step 5 not done), or too cold. Warm the room to about 20 °C. Milky white cloud in the solution from the start → your water contains salt (chloride). Use distilled water. Speculum cracked in cooling → cooled too fast. Bury it in hot ash; cast thicker.

Dangers

Danger Silvering solution left standing can explode. Silver nitrate mixed with ammonia, especially with caustic potash, slowly forms black crystals ("fulminating silver") that can blow up at a touch when they dry out — on a jar rim, in a crust on a dish. Mix it only immediately before use. Never store it. Never let it dry anywhere. Pour every leftover into a bucket of water with a good handful of salt and a cup of vinegar stirred in: the acid breaks up the silver–ammonia compound and the silver drops out as harmless white silver chloride (which you can save and turn back into silver, Silver Nitrate and Silver Salts). Wash all glassware at once.

Warning Caustic potash and strong ammonia burn skin and eyes; nitric acid burns worse (Lye and Potash, Ammonia, Nitric Acid). Wear something over your eyes. Work outdoors or by an open window — ammonia fumes choke. Silver nitrate stains skin black for days and is poisonous to swallow.

  • Mercury. Do not make amalgam mirrors; handle broken old mirrors over a tray and collect any droplets (Mercury).
  • Molten metal and crucibles: see Metal Casting and Bronze. Never pour onto damp ground.
  • Concentrated sunlight. A concave mirror — even a shaving mirror — on a sunny windowsill can start a fire; large dishes burn skin and blind in an instant. Cover them when not in use. Never look into the focus.
  • Glass edges: grind or file the edges of every mirror smooth.

Going further

How it was first done

The oldest known mirrors are polished discs of obsidian, volcanic glass, from Çatalhöyük in Turkey, about 8,000 years old. Polished copper mirrors were used in Egypt and Mesopotamia by about 3000 BC, and bronze mirrors in China from about 2000 BC; Chinese mirror makers became masters of high-tin bronze, with richly cast backs. Roman glassmakers made small mirrors of glass backed with lead. Glass mirrors backed with tin-mercury amalgam were perfected in Venice in the 1500s and were for two centuries among the costliest objects in Europe. Isaac Newton ground a speculum mirror for his reflecting telescope in 1668. In 1835 the German chemist Justus von Liebig discovered how to deposit silver on glass from a silver solution with a sugar, and by the 1850s Carl August von Steinheil and Léon Foucault were silvering glass telescope mirrors. John Brashear in Pittsburgh published his improved silvering formula in the 1880s. In 1932 John Strong coated telescope mirrors with aluminium in a vacuum, the method used today.

Source: content/entries/knowledge/mirrors.md