◆ Rebuild

Part 3 · Metals

Tins, Cans, Drums and Tanks

The family of sheet-metal containers that hold, carry and keep things — soldered and double-seamed food cans, tin boxes with lids, bottle caps, buckets and pails, watering cans, funnels, canteens, jerrycans, oil drums, water tanks and metal foil. How to lay each out, close its seams, and tell a tight one from a leaker.

Difficulty
●●●●●
Time
An hour for a soldered can or funnel once you have tinplate; a day for a watering can; several days for a drum or a riveted tank
Steps from zero
21 prerequisites →

You need first

Sheet Metal and RollingSoldering and BrazingTin and Pewter

This unlocks

—
The full path from nothing — 21 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. The Wheel and Axle
  12. Bellows
  13. Gears
  14. Iron (the Bloomery)
  15. Tin and Pewter
  16. Lead
  17. Copper Smelting
  18. The Waterwheel
  19. Blacksmithing
  20. Soldering and Brazing
  21. Sheet Metal and Rolling
  22. Tins, Cans, Drums and Tanks

Do them roughly in this order. See it on the tech tree →

Why it matters

A clay pot breaks, a barrel leaks when it dries, a leather bag rots. A sheet-metal container is light, survives being dropped, can be sealed airtight and can go on a fire. Once you can make thin sheet (Sheet Metal and Rolling), coat it against rust (Tin and Pewter) and seal seams (Soldering and Brazing), a whole family follows: cans that keep food for years (Canning and Bottling); tin boxes that keep tea, matches, medicine and seed dry and safe from mice; buckets, pails and watering cans for the house, the animals and the garden; funnels and canteens; jerrycans and drums that store and move fuel, oil and water by the hundred litres; tanks for a village water supply; and foil for wrapping and for capacitors.

All are made the same way: lay out a flat pattern, cut it, bend it, close the seams. This chapter covers what is particular to each; sacks, crates and cartons are in Sacks, Boxes, Crates and Packaging.

How it works

Every container is flat pieces joined at seams. A cylinder unrolls into a rectangle; a cone or tapered bucket into part of a ring (see the bucket layout in Sheet Metal and Rolling); an end into a disc.

Soldered lap small cans, lids 3–5 mm solder fillet Lock seam hooks 6 mm, hammered flat hook of A hook of B solder only seals it Wired edge stiff, safe rim wire allowance 2½ × wire Double seam (can end), in three stages grey = tinplate; the can spins on a chuck while each roller is pressed in 1. Ready body flange lid panel compound can wall 2. First roller deep groove curls lid under flange roller 3. Second roller flat groove presses tight 5 layers, about 3 mm tall chuck inside lid
Fig. 1 Four seams in cross-section. The soldered lap is simplest; the lock seam holds without solder; the wired edge stiffens a rim; the double seam closes a can or drum end in two rolling steps with no solder at all.
  • Soldered lap: edges overlap 3–5 mm and are sweated together. The solder carries the load, so it suits only small things.
  • Lock seam: each edge folded into a hook, interlocked and hammered flat. The folds hold; solder only seals.
  • Wired edge: the rim rolled round a wire, for stiffness and safety.
  • Double seam: the lid's edge curled under a flange on the body and rolled tight into five interlocked layers, sealed by a thin rubbery compound. Airtight with no solder; used on nearly every can and drum end since about 1900.

Thin sheet is floppy flat but stiff when curved. That is why containers are round where they can be, and why flat panels get rolled beads, ribs or a pressed X (as on a jerrycan).

Water pressure grows with depth: about 10 kPa (0.1 bar) per metre. The bottom ring of a tank works hardest. For round tanks use the boiler rule in Sheet Metal and Rolling: thickness = pressure × diameter ÷ (2 × allowable stress × joint efficiency).

Bare iron rusts. Coat it with tin for anything touching food; zinc (hot-dip galvanising, Electroplating) for buckets, tanks and roofing, but never for acid food; or Enamel on Metal, paint or tar. See Corrosion and Its Prevention.

What you need

Item Notes
Sheet Tinplate 0.2–0.4 mm for cans, boxes, caps, funnels; tinned or galvanised iron 0.5–0.8 mm for buckets and watering cans; steel 0.9–1.2 mm for jerrycans and drums; plate 1.5–3 mm for tanks
Solder and flux Pure tin (or tin with a little copper or antimony) for anything touching food or drinking water; rosin or zinc chloride flux (Soldering and Brazing)
Tools Snips (Scissors, Shears and Folding Knives), mallets, stakes, mandrels, folding bars, groover, rivet set, soldering irons, scriber, dividers, a cord and nail for big arcs
Wire and rivets Iron wire 1.5–5 mm (Iron and Brass Wire); tinned iron or copper rivets 3–8 mm (Nails, Rivets and Wire Fasteners)
Sealing compound Rubber solution (Rubber), or a paste of linseed oil and chalk
For drums, cans by the thousand A The Lathe or rolling machine; ideally a press and Welding

Where to find it

Iron sheet comes from Sheet Metal and Rolling, tin from cassiterite stream pebbles (Tin and Pewter), rosin flux from pine resin (Tar, Pitch and Glue), stoppers from cork bark or turned hardwood; wet sand scours sheet bright before tinning and soldering. Salvaged drums and roofing iron are the richest store of ready sheet in any ruin — one drum opened out gives nearly 2 m² of steel — but everything below starts from sheet you can make yourself.

Food cans

The soldered can

This is the can of 1810–1900, and the one to make first. A useful size is 75 mm across and 110 mm tall (about 450 ml); smaller cans heat through faster when processed, which makes them safer.

  1. Body. Cut tinplate π × diameter + 5 mm long (241 mm for 75 mm) and the can's height + 6 mm wide. Roll it on a mandrel, lap 5 mm and solder the seam on the outside.
  2. Flange. Turn out 3 mm at each end over the edge of a round stake.
  3. Ends. Cut discs 6 mm bigger than the can, turn up their rims 3 mm over a wooden former, fit them, fold the rims down over the flanges and solder round. Punch a filling hole 25–30 mm across in the top.
  4. Fill and close. Fill, leaving 6–10 mm headspace, solder on a cap with a pinhole vent, process (see Canning and Bottling), and close the vent with a drop of solder while hot.

Use lead-free solder and rosin flux on every joint that touches food.

The double-seamed can

A can seamer spins the can and presses two rollers in turn against the joint. Build one on a The Lathe.

  1. Body as before, but with a flange only 2–2.5 mm wide at each end.
  2. Lid. Press a disc about 12 mm larger than the can, in a wooden or iron die, into a shallow cup: a flat panel, a ring-shaped step (the countersink) 3–4 mm deep that fits inside the body, and a rim curled down at the edge. Run a bead of sealing compound inside the curl and let it dry.
  3. Chuck. Turn a hardwood or iron disc that fits exactly inside the countersink and mount it on the spindle; a pad on the tailstock presses the can against it.
  4. First roller: hardened steel, 25–40 mm across, with a deep, narrow, rounded groove. Pressed against the spinning rim, it curls the lid's edge in under the body flange.
  5. Second roller: a shallow, flat groove. It irons the hooks tight. The finished seam is about 3 mm tall and 1.2–1.5 mm thick for 0.2–0.25 mm plate.

Tip Saw a finished end across and look at the cut with a magnifier. You want five layers, hooked deeply together. Hooks barely overlapping: press the first roller in further. Fat, loose seam: press the second harder.

The aluminium can (in outline)

The modern drinks can is two-piece: a disc of aluminium alloy about 0.3 mm thick is drawn into a cup, then forced through rings that iron the wall down to about 0.1 mm, while the bottom stays thick and is domed against pressure. The top is necked in and a stiffer lid (about 0.22 mm) is double-seamed on. A 330 ml can is about 66 × 115 mm and holds 5–6 bar. The inside is lacquered because acid drinks attack aluminium. It needs Aluminium in quantity, rolling held to thousandths of a millimetre, and presses making hundreds a minute — not a first-generation object.

Tin boxes with lids

The commonest is a cylinder with a slip lid that slides over the body.

  1. Body: a cylinder with a bottom, its top edge wired, beaded or folded in 3 mm so the lid slides on something smooth.
  2. Lid: a short cylinder 15–20 mm deep whose inside diameter is the body's outside plus 0.3–0.5 mm. Wrap its blank round the finished body over one layer of paper as a spacer, mark the overlap, solder, then solder on a top.
  3. Fit: a good lid slides on with a faint sigh of air and does not fall off when the box is held upside down. Too loose: tap its rim in on a stake. Too tight: stretch it on a mandrel.

Square boxes fold from one piece with corner tabs soldered inside. For a hinge, roll 4–5 mm tubes from alternating tabs on box and lid and push a wire through. Plug (lever) lids, as on a paint tin, push into a raised ring; cut ring and plug wall from the same strip so they match.

Bottle caps and crown caps

A crown cap is a tinplate disc with a fluted skirt crimped under a bead round a bottle's mouth, with a cork liner that seals against the glass. It holds the pressure of beer or soda water (Beer, Wine and Cider).

The crown cap holds the pressure of beer or soda water 21 flutes Pressed cap tinplate 0.2–0.25 mm cork liner about 32 mm Capping bell mouth tapers 32 → 28.5 mm bead 26 mm Crimped under bead One firm mallet blow on the bell folds the skirt in. The watering can 8–10 litres Rose 150–300 holes, 1 mm filling hole spout tip above brim handle water level brace Spout set low, tapers 30 → 15 mm
Fig. 2 Left: the crown cap. A disc of tinplate is pressed into a fluted cup with a cork liner; a capping bell, struck once, folds the flutes under the bottle's bead. Right: a watering can. The spout joins low down but its tip rises above the brim, so the can does not empty itself when full.
  • Sizes: bottle bead about 26 mm across (Glass); disc of 0.2–0.25 mm tinplate about 37 mm, pressed into a cup about 32 mm across and 6 mm deep with 21 flutes.
  • Making: an iron die with a 21-grooved round hole and a matching punch, struck with a heavy mallet or a screw press. Glue in a cork disc 2–3 mm thick.
  • Capping: a capping bell — a steel tube whose mouth tapers from 32 to about 28.5 mm — set over the cap and struck once. All flutes should tuck evenly; one side standing out means the bell was not square.

Before crown caps came corks wired down, and the reusable swing stopper: a porcelain or wooden plug with a rubber ring, pulled down by a wire lever. Make that first if you have wire and rubber. Screw caps are pressed from tinplate with a rolled thread, or turned from wood (Screws, Nuts and Bolts).

Buckets and pails

The layout and seams of a tapered bucket are in Sheet Metal and Rolling. What makes a metal bucket last:

  • Sheet 0.5–0.8 mm, tinned or galvanised. A 10-litre bucket (30 cm top, 24 cm bottom, 25 cm tall) takes about 0.3 m².
  • Bottom of heavier sheet than the body, set 5–10 mm up inside, so the folded edge of the body takes the wear, and soldered from inside.
  • Rim wired with 4–5 mm wire, or it folds in the first time a full bucket is knocked.
  • Ears of 1.5 mm iron riveted below the rim with two rivets each; a bail of 5–6 mm rod, with a wooden roll for the hand.

A pail is a straight or slightly tapered bucket with a pouring lip pressed out of the rim and often a lid. Milk pails must be tinned, never galvanised — souring milk dissolves zinc (Dairy and Cheese).

Watering cans

A watering can gives a gentle shower that does not wash seed out of the soil.

  1. Body: a round or oval drum 20–25 cm across and 25–30 cm tall (8–10 litres, about 10 kg full). Close most of the top, leaving a filling opening at the back.
  2. Spout: a cone 50–60 cm long, 30–35 mm across at the body and 15–20 mm at the tip, rolled on a tapered wooden former. Solder it in low on the front, sloping up so its tip is above the brim — or the full can empties through it. Brace it halfway with a strap.
  3. Rose: a short cone 6–10 cm across with a domed face of thin brass or tinplate, pierced with 150–300 holes of about 1 mm (punched from inside over end-grain wood); 1.5–2 mm holes for grown plants. It slips over the spout.
  4. Handle: a strip of 1.5 mm sheet with folded edges, arched from top to back, soldered and riveted.

A good one pours an even shower from every hole and balances in the hand when full.

Funnels

A funnel's cone is laid out exactly like a bucket side. A household funnel: 15 cm across, sides at 60° to each other, a spout 12–15 mm across and 6–8 cm long cut off at a slant. Solder a narrow strip down the outside of the spout: it lets air out of the bottle, so the funnel does not glug and overflow. Wire the rim and add a ring for hanging.

Canteens

A canteen of about 1 litre: dish two discs of tinplate, tinned iron or copper 0.5–0.6 mm thick and about 17 cm across to 3–4 cm deep over a hollow in a hardwood stump. Join them rim to rim with a strip folded over both edges and soldered. Solder in a neck 20–25 mm across, closed by a cork or turned wooden stopper on a cord. Sew on a cover of wool felt (Felt): soaked, it cools the water by evaporation and stops the metal burning the hand. Rinse canteens and dry them open, or they grow slime.

Jerrycans

The jerrycan holds 20 litres in a flat steel can about 47 × 34 × 16 cm, 4 kg empty.

The 200-litre oil drum bungs: 50 mm and 20 mm Chime double seam Rolling hoops at ⅓ and ⅔ rolls on these, not the wall welded or riveted seam steel 0.9–1.2 mm about 57 cm 85–88 cm The jerrycan 20 litres, 47 × 34 × 16 cm cam-lever cap Three handles breather tube air space, liquid stops here Pressed X stiffens the flat side two halves, welded round the edge
Fig. 3 An oil drum and a jerrycan. The drum's rolling hoops let one person roll 200 kg; the jerrycan's three handles, pressed X and air space make it strong, easy to pass and easy to pour.

Its features are worth copying: two pressed halves welded round the edge, so there is no bottom seam to leak; an X pressed into each side to stiffen it and let it flex as the contents expand; three handles so one person carries it, two can pass it, or one can carry two empties; an air space under the handles for expansion, which also makes a full can float; and a cam-lever cap with a rubber gasket and an internal breather tube, so it pours without glugging. It needs a press, 1 mm steel and Welding.

The workshop version is the square four-gallon tin that carried kerosene and water before it: a box 24 × 24 × 35 cm of 0.3–0.4 mm tinplate, lock-seamed at the corners, with beaded sides, a wire handle and a screw-capped spout in one corner of the top. It dents easily but holds 18 litres and needs only snips, folding bars and solder.

Oil drums

The standard drum holds 200 litres, about 57 cm across and 85–88 cm tall; full of water it weighs about 220 kg. Its parts:

  • Body: one sheet of 0.9–1.2 mm steel, about 180 × 88 cm, rolled and seam-welded.
  • Rolling hoops: two ridges about 15 mm high at one-third and two-thirds of the height, rolled out between grooved rolls (Sheet Metal and Rolling). They stiffen the body and take the wear when it is rolled.
  • Heads: 1–1.2 mm discs double-seamed on, leaving a raised rim (the chime) that protects the head when dropped.
  • Bungs: threaded holes of about 50 mm (pouring) and 20 mm (air) with screwed plugs and washers.

A first drum without a welder: roll the body in two or three rings, rivet the laps with 5 mm rivets at 25 mm spacing and solder or caulk; flange the heads over a wooden former and rivet and solder them 2 cm inside the body ends, so the body forms the chime; rivet on two flat iron hoops as on a barrel (Barrels and Cooperage). For water and oil, it serves.

Water tanks

A tank stores roof water or pumped well water (Wells and Cisterns, Pumps).

  • Riveted round tank. A tank 3 m across and 2 m tall holds about 14,000 litres. At the bottom the water pushes with 0.02 MPa, so with an allowable stress of 50 MPa and a riveted joint efficiency of 0.6, strength needs only 1 mm plate. Use 2–3 mm for the bottom ring and 1.5–2 mm above, because rust, not strength, decides its life. Rivets 6–8 mm at three to four diameters' spacing; caulk the edges.
  • Corrugated tank. Galvanised corrugated sheet 0.5–0.8 mm bent into a cylinder 1.5–4 m across, riveted and soldered, on a flat bottom bedded on sand over a stone or concrete base. The corrugations stiffen the thin wall. Limewashed or tarred inside and kept off wet soil, it lasts 15–30 years.
  • Sectional tank. Square panels about 1.2 m on a side with flanged edges, bolted flange to flange over a gasket of tarred hemp, rubber or felt, with tie rods across the inside. It travels in pieces and can be enlarged.

Every tank needs a lid (against light, which grows algae, and mosquitoes), a screened overflow, an outlet 5–10 cm above the floor so sludge stays behind, a drain at the lowest point, and a base that cannot settle unevenly.

Metal foil

  • Tin foil. Cast a slab 5 mm thick, roll it cold in a hand mill (Sheet Metal and Rolling), then fold and roll it double, again and again, dusted with chalk so the layers part. A hand mill reaches 0.02–0.05 mm. Tin needs no annealing.
  • Aluminium foil is rolled hot, then cold through many passes with annealing, and the last pass is made two sheets at once — which is why one side is dull. Kitchen foil is 0.016–0.024 mm.
  • Beaten foil: gold beaten between skins becomes leaf 0.0001 mm thick (Gold and Silver); tin and copper can be beaten too, but rolling is far quicker.

Never wrap food in lead foil or tin foil containing lead.

How to tell it worked

  • Water test: fill to the brim and stand on dry paper overnight. Mark wet spots, dry, clean and re-solder.
  • Bubble test for closed vessels: blow gently into it through a tube and brush soapy water on every seam. Never use high-pressure air — a failing seam throws the end off. Test strong vessels full of water (Sheet Metal and Rolling).
  • Processed cans: both ends drawn slightly inward, and the centre does not click when pressed.
  • Seam section: five well-hooked layers in a double seam; solder right through a lap with no dry spots.
  • Drop test: a full canteen or bucket dropped from waist height onto earth may dent but must not leak.

Note Troubleshooting. Solder balls up → metal dirty or not hot enough. Scrape bright, re-flux, and let the iron heat the work. Can end bulges after a week → leaking seam or under-processing. Do not taste it; bury it (Canning and Bottling). Double seam leaks at one spot → the side-seam lap is too thick where it crosses. File its ends thin before seaming. Bucket bottom leaks after weeks → flexing cracked the solder. Set the bottom up inside and fold it in, so the fold carries the load. Watering can dribbles → spout tip below the water level. Make it longer or set it steeper. Tank bulges at the bottom → plate too thin or rivets too far apart. Add an iron hoop round the outside.

Dangers

Danger Never cut, weld, braze, solder or grind a drum, can or tank that has held fuel, oil, solvent or an unknown chemical. Vapour left inside — even when it looks and smells empty — explodes in the heat and blows the end off with lethal force. If you must repair one, wash it out with hot soda water many times and then fill it with water to just below the work. Keep your body out of line with the ends.

Danger Lead in food and water. Tin-lead solder, lead-coated "terne" plate and lead foil leach lead, especially into acid food. Lead poisoning is slow, invisible and permanent, and harms children most. Use pure tin for every joint touching food or drinking water. See Lead.

  • Galvanised fumes. Heating zinc-coated iron to red heat gives white fumes that cause metal fume fever — a day of flu-like shivering. Work outdoors or scrape the zinc off first.
  • Zinc chloride flux burns skin and eyes. Wash every trace off; never use it inside food cans.
  • Cut edges are razors. File every burr; wire or fold every edge that hands touch.
  • A full drum weighs over 200 kg. Roll it on its hoops, tip it with a lever and a helper, never stand downhill of it.
  • Unknown containers may have held poison. Do not use them for food or water.

What this unlocks

Cans make Canning and Bottling work on a large scale, feeding travellers, armies and cities through winter. Drums and jerrycans let you store and move Petroleum and Refining products, chemicals and water, so The Internal Combustion Engine engines and tractors can work far from a refinery. Tanks underpin village water supplies (Water Treatment for a Town, Pipes, Plumbing and Aqueducts). The same skills make lanterns (Lamps and Candles), cooking pots (Pots, Pans and Kettles) and Kitchen Utensils and Gadgets.

How it was first done

Tinplate was made in Bohemia and Saxony by the 14th–15th centuries, and at Pontypool in Wales from about 1720. In 1810 Peter Durand patented food in tinned iron cans, following Nicolas Appert's bottling method; by 1813 Donkin and Hall supplied the Royal Navy. Early cans were soldered by hand — a good tinsmith made perhaps sixty a day — and opened with hammer and chisel. The double-seamed "sanitary" can, sealed with compound instead of solder, came in the 1890s and spread after the Sanitary Can Company was founded in New York in 1904.

William Painter of Baltimore patented the crown cap in 1892. The 200-litre steel drum descends from a steel barrel patented in 1905 and made at the ironworks owned by the journalist Nellie Bly. The jerrycan was designed in Germany in 1937 for the army; Allied soldiers copied it and named it after the "Jerries" they took it from. John Haws patented his long-spouted watering can in London in 1886. Continuous rolling of aluminium foil began in Switzerland in 1910, and the aluminium drinks can went on sale in the United States in 1959.

Source: content/entries/metals/tins-cans-and-drums.md