◆ Rebuild

Part 2 · Earth and Fire

Glazes

A glaze is a thin skin of glass melted onto a pot. It makes pottery waterproof, easy to clean and beautiful. This chapter covers slips, glass-powder glazes, ash glazes and salt glazing, colouring with iron, copper and cobalt, firing, faults — and why lead glazes must never touch food.

Difficulty
●●●●●
Time
A day to prepare ingredients; a week or more of test firings before a reliable glaze
Steps from zero
7 prerequisites →

You need first

PotteryGlass

This unlocks

Pyrometric Cones and Kiln TemperatureStoneware and PorcelainEnamel on Metal
The full path from nothing — 7 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Pottery
  4. The Kiln
  5. Lime
  6. Lye and Potash
  7. Glass
  8. Glazes

Do them roughly in this order. See it on the tech tree →

Why it matters

Unglazed earthenware is porous. It sweats water, soaks up fat and milk until they go rancid, holds germs in its pores, and slowly lets wine and vinegar seep away. A glaze — a thin layer of glass fused onto the surface — fixes all of that:

  • Waterproof and clean. A glazed jar holds oil, milk, honey, pickles and wine for years. A glazed bowl can be scrubbed clean, which matters for health (see Sanitation and Germs).
  • Acid- and chemical-resistant. Good glazes resist vinegar, fruit juice and most chemicals — essential for Preserving Food, Fermentation, Dyes and Mordants and the work in Acids, Bases and Testing.
  • Stronger and more beautiful. Glaze adds strength, colour and shine.

Glazes lead on to glazed Tiles and Clay Pipes, to Stoneware and Porcelain — the dense, glassy ware of laboratories and kitchens — and to the porcelain insulators of electrical wiring.

How it works

A glaze is simply glass (see Glass) that is ground to powder, painted onto a pot, and melted in the The Kiln so it flows into a smooth skin. Like any glass, it needs three kinds of ingredient:

Job What it does Natural sources
Glass-former (silica) Makes the glass. Alone it melts only at 1,710 °C Quartz, sand, flint, clay
Flux Lowers the melting point to something a kiln can reach Wood ash (potash and lime), plant-ash soda, limestone, feldspar, salt; also lead (dangerous)
Stiffener (alumina) Makes the melted glaze thick so it does not run off the pot; helps it grip Clay, feldspar

Two numbers rule every glaze:

  1. Melting temperature. The glaze must melt at a temperature the pot survives. Ordinary red earthenware is fired to about 950–1,100 °C; the glaze must melt below that, which needs a strong flux. Stoneware is fired at 1,200–1,300 °C (see Stoneware and Porcelain), where plain wood ash and clay melt into glaze.
  2. Fit. When the pot cools, the glaze and the clay shrink. If the glaze shrinks more than the clay, it is stretched and cracks into a fine network (crazing). If it shrinks less, it is squeezed and flakes off the edges (shivering). More silica in the glaze — or more sand in the clay — makes the glaze shrink less. More alkali (ash, soda, potash) makes it shrink more.
Silicaquartz, sand, flintmakes the glass Fluxash, lime, feldspar, saltlowers the melting point Clay (alumina)stiffens the meltstops it running off ground fine, mixed with water, melted in the kiln Glaze, about 1 mmsmooth glass skin Bond layerglass soaked into clay Pot wallfired clay with pores
Fig. 1 A glaze is a skin of glass. Silica makes the glass, flux makes it melt at kiln heat, and clay stiffens it. Where the glass bonds into the clay surface it forms a thin middle layer that holds it on.

What you need

Item Notes
Bisque-fired pots Pots already fired once to about 800–900 °C — still porous, so they soak up glaze. See Pottery and The Kiln
A kiln that reaches the glaze's melting heat 1,000–1,100 °C for glass-powder glazes; 1,200–1,280 °C for ash and salt glazes
Grinding stones A flat stone and a hand stone, or a quern (see Grain, Flour and Bread) used only for glaze — never for food
Sieves Finest cloth you have (linen or silk); glaze must be fine as flour
A balance Measure ingredients by weight. A beam balance with stones of known weight works (see Measurement from Scratch)
Buckets, jars, a stirring stick Kept only for glaze
Test tiles Dozens of small flat pieces of bisque, 5 × 10 cm, with a hole to hang them

Where to find it

  • Wood ash — from any hearth; hardwood ash is best. Each kind of wood gives a slightly different glaze. See Lye and Potash.
  • Quartz and sand — white quartz pebbles, heated red-hot and dropped in water so they crack, then ground; or the cleanest, whitest sand.
  • Clay — your ordinary pottery clay, or a pale clay for a lighter glaze (see Finding and Preparing Clay).
  • Feldspar — pink, white or cream crystals in granite, often the largest crystals in the rock, with flat shiny faces that catch the light. It is a natural glaze on its own at about 1,250–1,300 °C.
  • Limestone, chalk, seashells — ground to powder, a strong flux at stoneware heat (see Lime).
  • Colours:
    • Iron — red ochre, rust, red or brown iron ore (hematite), or the red clay itself.
    • Copper — the black scale that flakes off copper heated in a fire (see Copper Smelting), or crushed green malachite.
    • Cobalt — rare. Look for pink to purple crusts ("cobalt bloom") on rocks in old silver, nickel and copper mining districts. A tiny amount gives a strong blue.
    • Manganese — soft black ore that blackens fingers, often as fern-like black patterns on rock faces.

Slips: the first step

A slip is clay thinned with water to the consistency of cream. It is not glass, but it changes the surface:

  • White or coloured slip. Dip or paint a red pot with slip made from a pale clay; it fires cream or white, a clean ground for painted decoration. Add iron ore for a red-brown slip.
  • Terra sigillata — the glossy red surface of Roman tableware. Mix clay with about four times its volume of rainwater, add a pinch of Lye and Potash or plant ash, stir well and leave for one to two days. Pour off the cloudy middle layer, leaving the coarse sludge at the bottom. Let the cloudy water settle again, or boil it down, until it is like thin milk. Brush two or three thin coats onto a bone-dry pot, and polish with a soft cloth or a smooth stone. Fired to 900–1,000 °C it gives a satin shine that reduces porosity — not fully waterproof, but much better than bare clay.

Method 1: Glass-powder glaze (the easiest true glaze)

Since a glaze is just glass, the simplest route is to make glass first (see Glass) and grind it. This is what early Near Eastern potters did with their "frit". Melting it once beforehand also locks up the soluble ash, which otherwise dissolves in the glaze water.

  1. Grind the glass. Crush clean glass (broken pieces or a failed melt) on a flat stone, wearing a damp cloth over your face. Grind with water until it is fine as flour and passes your finest cloth.
  2. Mix, by weight: 85 parts glass powder to 15 parts clay. The clay keeps the glaze from settling hard in the bucket and helps it stick and stay put on the pot.
  3. Add colour if wanted (see the table below).
  4. Add water until it is like single cream — a finger dipped in it should come out coated, so you can just not see the skin through it.
  5. Apply and fire to 1,000–1,100 °C (orange to yellow-orange heat).

This glaze is shiny and colourful, but soda and potash glasses shrink a lot, so on ordinary clay it usually crazes. For water jars and decoration that is acceptable. To reduce crazing, add up to 15% fine quartz to the glaze, or more fine sand to the clay body.

Method 2: Ash glaze (stoneware)

Wood ash and clay make one of the oldest and loveliest glazes — but only at stoneware heat, 1,220–1,280 °C (yellow to white glow). An ordinary wood kiln cannot do it; you need a hotter kiln (see Stoneware and Porcelain).

  1. Wash the ash. Soak sieved ash in plenty of water, stir, let it settle, and pour off the water. Repeat two or three times. This removes the caustic, soluble part (wear gloves or grease your hands — wet ash burns skin; see Lye and Potash).
  2. Dry and sieve it through fine cloth.
  3. Mix, by weight: 1 part ash to 1 part clay as a start. If it is dry and rough after firing, use more ash; if it runs off the pot, use more clay. Adding feldspar (for example 40 ash : 40 feldspar : 20 clay) gives a smoother, more reliable glaze.
  4. Apply thinly and fire.

Ash glazes run in streaks and drops and turn green, amber or blue-grey depending on the iron in the ash and clay. In long wood firings, ash flying from the fire settles on pots and melts into a natural ash glaze on its own — this is how the glaze was first discovered.

Method 3: Salt glazing (stoneware)

Here the glaze is made inside the kiln. At 1,200–1,280 °C, throw damp common Salt into the firebox. It turns to vapour, the sodium in it combines with the silica in the hot clay surface, and every pot is coated with a thin, hard, glassy skin with a texture like orange peel.

  1. Fire unglazed stoneware (no bisque needed) to full heat.
  2. Throw in salt, a few handfuls at a time through the stoke holes or special ports, every 10–15 minutes over about an hour. Use roughly 8–15 kg of salt per cubic metre of kiln space in total.
  3. Pull out a draw trial — a small ring of clay placed where you can hook it out — after each few doses. Stop when it is glossy.

Salt glaze needs no grinding or dipping, and it is extremely tough and acid-proof — ideal for storage jars, bottles and drain pipes. But the kiln walls get glazed too, and the fumes are dangerous (see Dangers).

Lead glazes, and why to avoid them

For two thousand years, most low-fired glazed pottery in Europe and the Middle East used lead: powdered lead ore (galena) or lead oxide mixed with sand and clay melts at only 900–1,000 °C into a smooth, shiny, honey-yellow glaze (green with copper). It is easy, and it fits earthenware well.

But lead dissolves. Acid foods — wine, vinegar, fruit, pickles, sour milk, tomatoes — pull lead out of the glaze, and the eater slowly accumulates it. Lead poisoning causes stomach pain, anaemia, kidney damage, infertility, and permanent brain damage in children. There is no simple test to tell a "safe" lead glaze from an unsafe one.

Rule: never use lead glaze on anything that touches food or drink. If you use it at all — for roof tiles, drain pipes or flowerpots — keep the raw materials away from kitchens and children, and wash carefully. Treat old shiny yellow, green or brown pottery from ruins as suspect.

Colours

Add colourants to the dry glaze by weight:

Colourant Amount Colour in clean, airy fire Colour in smoky fire (reduction)
Iron (ochre, rust) 1–2% Pale honey, amber Pale green-blue (celadon)
Iron 4–6% Brown Olive green
Iron 8–10% Dark brown to black Black, rust-red edges
Copper scale or malachite 1–3% Green (turquoise in soda or potash glaze) Red (difficult)
Cobalt ¼–1% Strong blue Blue
Manganese 2–6% Purple-brown Brown
Tin oxide 5–10% Opaque white —

Smoky fire (reduction) means firing with too little air at the end, so the flame is lazy and smoky and pulls oxygen out of the colourants. Clean, airy fire (oxidation) means plenty of air and clear flames.

For painted decoration, mix the colourant with a little water and gum, paint it onto the raw glaze or onto the bisque under a clear glaze. Cobalt blue painted under a clear glaze is the famous "blue and white" ware.

Step by step: glazing a pot

  1. Bisque-fire your pots to about 800–900 °C (bright cherry red). They are hard enough to handle but still porous.
  2. Clean them. Brush off dust and do not touch the surfaces with greasy hands — grease and dust make the glaze crawl away.
  3. Stir the glaze thoroughly; it settles fast.
  4. Glaze the inside first: pour the pot half full, swirl, and pour out, turning, in about 3 seconds.
  5. Glaze the outside: hold the pot upside down by the foot and dip it straight down into the bucket for 2–3 seconds. The glaze coat should be about 1 mm thick — about as thick as a fingernail. Too thin gives a dry, rough surface; too thick runs, crawls or crazes.
  6. Clean the foot. Wipe all glaze off the base and 5 mm up the side with a damp cloth. Melted glaze glues pots to the kiln floor and to each other.
  7. Dry for a day.
  8. Load the kiln with a finger-width gap between glazed pots. Stand each on clean, unglazed ground or on little pads of clay mixed with sand (wadding) or three-legged clay stilts.
  9. Fire to the glaze's melting heat (see The Kiln for the schedule and colours). Put glazed draw trials — small rings dipped in the same glaze — where you can hook them out through a spy hole. When a trial, pulled out and cooled, is smooth and glossy, hold the heat for 20–30 minutes, then close up.
  10. Cool slowly. Opening early cracks both pots and glaze.
1. Dip 2–3 seconds 2. Wipe the foot clean 3. Stand on a stilt glaze like single cream Bare clay5 mm up the side Glazeabout 1 mm Clay stilts Kiln floor
Fig. 2 Glazing a pot. Dip it for two or three seconds to coat it about 1 mm thick, wipe the foot clean, and stand it on stilts or wads so melted glaze cannot glue it to the kiln floor.

Test first. Always try a new glaze on test tiles before risking good pots. Make a row of tiles with the flux increasing step by step — for example ash : clay at 30:70, 40:60, 50:50, 60:40, 70:30 — and fire them together. Pick the one you like. Write every recipe down.

How to tell it worked

  • The glaze is smooth and glossy (or evenly satin), with no bare patches or pinholes.
  • Water test: fill the pot and leave it for a day on a dry stone. The outside stays dry.
  • Vinegar test: leave vinegar in it overnight. A good glaze keeps its shine; a poor one turns dull or rough.
  • Scratch test: a steel knife should barely mark a good glaze. Soft glazes scratch easily and wear through.
  • Tap the pot: it should ring.

Note Faults and fixes. Crazing (fine crack network) → glaze shrinks too much: add silica to the glaze, or sand to the clay; fire a little hotter. Shivering (glaze flakes off rims and edges) → the opposite: less silica, more flux. Crawling (glaze pulls into islands, leaving bare clay) → dusty or greasy bisque, glaze too thick, or too much raw clay in it; clean pots, apply thinner. Pinholes and blisters → gas escaping from clay or glaze: fire more slowly through the middle heats, and hold longer at the top so the glaze heals. Running down onto the shelf → too thick, too much flux, or overfired; add clay, apply thinner. Dry, rough, sandy surface → not melted: fire hotter or add flux. Wrong colour → the fire was smoky when it should have been clear, or the reverse.

Goodsmooth, glossy,even Crazingglaze shrinks toomuch: add silica Shiveringflakes off edges:less silica Crawlingdusty or greasy pot,glaze too thick Pinholesgas escaping: fireslower, hold longer
Fig. 3 Common glaze faults. Each has a cause you can read from its look.

Dangers

Danger Lead poisons slowly and permanently. Never use lead in glazes for anything that holds food or drink, and never grind lead ore where food is made. Lead dust and fumes from firing are also poisonous. Children are harmed most.

Danger Salt-glazing fumes. Salt in a hot kiln gives off choking hydrochloric acid gas, which burns eyes, throat and lungs. Salt-glaze only outdoors, far from homes, animals and crops, and stand upwind while dosing the kiln.

  • Silica dust. Grinding glass, quartz, sand and dry glaze makes fine dust that scars the lungs (silicosis). Grind wet, sweep wet, wear a damp cloth over nose and mouth, and work outdoors.
  • Cobalt ores often contain arsenic. Roasting them gives off a white smoke with a garlic smell — deadly poison. Roast only outdoors, upwind, and never breathe the fumes. Cobalt, copper and manganese powders are poisonous if swallowed: wash your hands and keep glaze tools away from food.
  • Wet ash is caustic. It burns skin and eyes like Lye and Potash.
  • Kiln heat and glare. See The Kiln.

What this unlocks

Glazed jars make safe Preserving Food and Fermentation vessels. Glazed Tiles and Clay Pipes last outdoors and carry water. Hotter firing and better clays lead to Stoneware and Porcelain, whose glazes resist almost every chemical — the start of a real laboratory. Glass powder fused onto metal makes enamel (Enamel on Metal); the same skills make coloured Glass and pigments.

How it was first done

The first glazes were on stone and on faience — a paste of crushed quartz and plant ash — in Egypt and Mesopotamia, from around 4000 BC, giving the turquoise blue of Egyptian beads and amulets. Glazed clay pottery appeared in Mesopotamia in the second millennium BC. In China, potters of the Shang dynasty (about 1500 BC) found that ash falling on pots in their hot kilns made a glaze, and began mixing ash glazes deliberately. Lead glazes were used in Han China and the Roman world by about 200 BC. Potters in 9th-century Iraq, trying to copy Chinese porcelain, invented white tin glazes and painted them with cobalt blue; the technique spread to Spain, Italy and the Netherlands (Delft). Cobalt was then traded back to China, giving rise in the 14th century to blue-and-white porcelain. Salt glazing was developed by stoneware potters in the Rhineland in Germany around 1400.

Source: content/entries/earth/glazes.md