◆ Rebuild

Part 3 · Metals

Titanium

Titanium is as strong as steel at little more than half the weight, and it shrugs off seawater, chlorine and the human body. Its ores lie in ordinary black beach sand, but the metal clings to oxygen, nitrogen and carbon so fiercely that it can only be made by turning it into a chloride and stripping the chlorine off with molten magnesium under inert gas. The easy prize comes first — titanium white, the brightest and safest white paint there is.

Difficulty
●●●●●
Time
A week to make your first kilogram of titanium white; titanium metal is a project of years for a settlement with power, chlorine, magnesium and argon
Steps from zero
29 prerequisites →

You need first

MagnesiumThe Electric Arc Furnace

This unlocks

—
The full path from nothing — 29 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Salt
  13. Bricks
  14. Fermentation
  15. The Wheel and Axle
  16. Firebrick and Refractories
  17. Bellows
  18. Gears
  19. Copper Smelting
  20. Iron (the Bloomery)
  21. The Waterwheel
  22. Blacksmithing
  23. The Battery
  24. Magnets
  25. Electrolysis
  26. Copper Wire
  27. Magnesium
  28. The Generator
  29. The Electric Arc Furnace
  30. Titanium

Do them roughly in this order. See it on the tech tree →

Why it matters

Titanium is the metal for jobs nothing else can do:

Be honest with yourself: the pigment is within reach of any settlement with Sulfuric Acid and a kiln. The metal is one of the hardest things in this book. It needs chlorine, magnesium, a supply of argon from liquid air, and electric furnaces, all working together.

How it works

Titanium is the ninth most common element in the Earth's crust — far more common than copper — but it holds on to other elements with terrible force:

  • Oxygen. Carbon cannot pull oxygen off titanium the way it does with iron (Iron (the Bloomery)). Heat titanium ore with charcoal, even in the arc furnace, and you get titanium carbide, a hard, brittle, useless crust — not metal.
  • Nitrogen and oxygen from the air dissolve in hot titanium. A few tenths of a per cent turn it as brittle as glass. Every hot step must happen in a vacuum or under argon (Liquid Air, Nitrogen and the Noble Gases).
  • Every crucible. Molten titanium (1,668 °C) dissolves clay, alumina, magnesia and graphite. It can only be melted in a water-cooled copper hearth, where a thin frozen skin of titanium itself forms the crucible.

The way round is the Kroll process:

  1. Turn the oxide into titanium tetrachloride (TiCl₄), a liquid that can be purified by distillation, by heating it with carbon in a stream of chlorine.
  2. Drip the liquid onto molten magnesium in a sealed steel vessel full of argon. Magnesium grabs the chlorine even more strongly than titanium does: TiCl₄ + 2 Mg → Ti + 2 MgCl₂. Titanium is left as a porous metallic sponge.
  3. Drive off the magnesium chloride, which goes back to the electrolysis cell to give magnesium and chlorine again (Magnesium).
  4. Melt the sponge into ingots in a vacuum or argon arc furnace with a water-cooled copper hearth.
Ilmenite or rutile sand Arc furnace 1,650–1,700 °C iron out as pig iron Chlorinator 900–1,000 °C TiO₂ + coke + Cl₂ Distil TiCl₄ clear liquid, boils 136 °C titania slag 75–85% TiO₂ Kroll reactor TiCl₄ onto molten Mg 800–900 °C, under argon Vacuum distil about 1,000 °C Mg and MgCl₂ boil off Arc melt water-cooled copper in vacuum or argon Titanium ingot sponge Magnesium cell molten-salt electrolysis MgCl₂ Mg chlorine goes round again Iron leaves twice: as pig iron from the arc furnace, and as iron chloride, condensed before the TiCl₄.
Fig. 1 The Kroll loop. Ore is concentrated, chlorinated with coke to titanium tetrachloride, distilled, and reduced by molten magnesium under argon to titanium sponge. The magnesium chloride is electrolysed back into magnesium and chlorine, which go round again.

Where to find it

Titanium ores are among the heavy minerals that collect with gold, tin and magnetite as black sand on beaches and in river bends (Finding and Identifying Ores, Gold and Silver).

  • Ilmenite (iron titanium oxide) — the main ore. Black grains or masses with a dull metallic shine, heavy (4.7 times water), black to brownish-black streak. Weakly magnetic: a lodestone barely moves it, but a strong The Electromagnet picks it up. Huge beach deposits in southern India (Kerala), eastern and western Australia, South Africa, Florida, Mozambique, Madagascar and Norway; also in dark igneous rocks (gabbro, anorthosite).
  • Rutile (titanium dioxide) — red-brown to black grains and needle-shaped crystals with a glassy, almost diamond-like lustre; pale brown streak; heavy (4.2); not magnetic. The golden hair-like needles in "rutilated" rock crystal are rutile. It is richer (about 95% TiO₂) but much rarer.

Concentrating black sand.

  1. Pan or sluice it as for gold (Gold and Silver) to throw off the light quartz.
  2. Dry it and sweep a weak magnet (a lodestone or a bar magnet wrapped in paper) through it to pull out the magnetite, which jumps to the magnet.
  3. Pass the rest under a strong electromagnet: ilmenite comes out next. What is left is mostly rutile, zircon (pale, glassy) and monazite (yellow-brown).

Testing for titanium. Dissolve a pinch of finely ground concentrate in hot strong sulfuric acid, cool, dilute with water, and drop in a piece of zinc. A violet colour appearing round the zinc within minutes means titanium.

Warning Monazite, the yellow-brown honey-coloured grains in some mineral sands, contains thorium and is mildly radioactive. Do not store large amounts of mineral-sand tailings in houses, and wash after handling them. See Detecting Radiation.

What you need

For titanium white (Method 1) For titanium metal (Method 2, in outline)
Ilmenite concentrate, ground to flour Rutile, or titania slag from ilmenite
Concentrated sulfuric acid, about 1.6 kg per kg of ore (Sulfuric Acid) Chlorine gas (Chlorine and Bleach) and coke (Coal and Coke)
Cast-iron or thick stoneware pot; scrap iron Magnesium metal (Magnesium)
Stoneware or wooden vats, cloth filters Argon (Liquid Air, Nitrogen and the Noble Gases) and a The Vacuum Pump
A kiln reaching yellow heat (The Kiln) Steel retorts, an The Electric Arc Furnace, water-cooled copper hearths

Method 1: Titanium white (the sulfate process)

This is how the first titanium pigment was made in Norway and the United States around 1916–1919, scaled down. From 1 kg of ilmenite (about 45–60% TiO₂) expect about 0.3–0.45 kg of pigment.

1. Digest 2. Leach cold 3. Reduce the iron 4. Freeze out iron 5. Boil to precipitate 6. Wash and roast ore + strong acid, 120 °C; a cup of water starts it; sets hard cake in cold water, keep below 60 °C scrap iron hung in it a day, until a faint violet tinge cool hard: green vitriol crystals grow; pour off liquid pour into boiling water, boil 3–4 h; white hydroxide settles wash until gall test stays clear; roast 800–1,000 °C, 2–3 h; grind: titanium white
Fig. 2 Titanium white from ilmenite. The ore is digested in sulfuric acid, leached with cold water, reduced with scrap iron, cooled to crystallise out green vitriol, then boiled to throw down white titanium hydroxide, which is washed and roasted.
  1. Grind the ilmenite concentrate to flour that feels smooth between the fingers (finer than 0.1 mm). Coarse grains do not react.
  2. Digest. Outdoors, in a cast-iron or thick stoneware pot, stir 1 kg ilmenite into about 1.6 kg (0.9 litre) of concentrated sulfuric acid to a thick slurry. Warm it gently to about 120–150 °C (it smokes and a stick dipped in it chars at once). Then stir in a small cup of water. The mass starts reacting by itself: it froths, steams, gets hotter (to about 200 °C) and in a few minutes sets into a solid, grey-green porous cake. Keep it warm for 2–4 hours to finish.
  3. Leach. Break the cake into lumps and soak it in about 4 litres of cold water, stirring, for several hours. Keep it below about 60 °C — warmer, and the titanium comes out of solution too early and is lost in the mud.
  4. Reduce the iron. Hang clean scrap iron (old nails) in the liquid for a day. It turns ferric iron (brown-yellow) into ferrous iron (pale green). When the liquid takes on a faint violet tinge, all the iron is ferrous. This matters: ferric iron would come down with the titanium and stain it yellow.
  5. Settle and filter off the black mud of undissolved ore through cloth.
  6. Freeze out the iron. Cool the clear liquid as cold as you can — a winter night, a cellar, or a pot in a bath of ice and salt (Ice and Refrigeration). Big pale-green crystals of green vitriol (iron sulfate) grow. Pour the liquid off them. Save the green vitriol: it is a valuable by-product for ink, dyes and other uses (Ink, Dyes and Mordants).
  7. Boil down the liquid to about two-thirds of its volume.
  8. Precipitate. Bring a small pot of clean water — about a quarter of the liquid's volume — to a rolling boil, pour the hot liquid slowly into it, then boil the mixture steadily for 3–4 hours, topping up with water. A fine white powder (hydrated titanium dioxide) settles out as the liquid clears.
  9. Wash. Let it settle, pour off the liquid, and wash the white sludge again and again with water — first with a little acid in it, then pure. Test the wash water with a few drops of oak-gall infusion (Ink): if it darkens, iron is still there; keep washing.
  10. Calcine. Dry the sludge, then roast it in a clean clay saggar in the kiln at 800–1,000 °C (bright orange to yellow) for 2–3 hours. It loses water and acid fumes, and becomes titanium dioxide. Below about 900 °C you get the anatase form, good indoors; roasted hotter and longer, with a pinch of rutile from a previous batch as seed, it turns to rutile, which lasts better outdoors.
  11. Grind the white lumps on a stone slab with a muller (Pigments, Paints and Varnish) and sieve.

Using it. Grind 1 part titanium white into about 0.4–0.5 part linseed oil for an opaque white oil paint. A little goes a long way: it hides the surface beneath far better than chalk, gypsum or even lead white, because it bends light more strongly than any other common white powder. It also whitens paper (Paper), makes white and opaque Enamel on Metal and Glazes, and is the coating on rutile welding rods (Welding).

Method 2: Titanium metal (the Kroll process, in outline)

Only attempt this when you already run chlorine, magnesium, argon and electric furnaces. Every step uses deadly chemicals at high heat. Expect years.

Step 1: A rich oxide

Rutile can go straight to chlorination. Ilmenite first goes to the The Electric Arc Furnace with about 10–12% of its weight of charcoal or coke. At about 1,650–1,700 °C the iron is reduced to liquid pig iron, which sinks, and the titanium stays oxidised in a titania slag of 75–85% TiO₂ floating on top. Tap both. (This is the route used in Quebec since 1950.)

Step 2: Chlorinate

Mix the crushed slag or rutile with about a third of its weight of crushed coke. Pack it into a vertical tower of silica brick or fireclay (Firebrick and Refractories), heated to about 900–1,000 °C (bright orange), and pass dry chlorine up through it. The titanium leaves as TiCl₄ vapour along with carbon monoxide and the chlorides of iron and other metals. Cool the gas in stages: iron chloride drops out first as a brown solid at about 200–300 °C, and TiCl₄ condenses as a yellowish liquid in a water-cooled condenser.

Step 3: Purify the "tickle"

Raw TiCl₄ (called "tickle") is yellow from vanadium. Stir it with copper turnings or a little mineral oil, then distil it in glass or steel (Distillation). Pure TiCl₄ is a clear, colourless liquid boiling at 136 °C. It smokes white in damp air as it reacts with water into hydrochloric acid and titanium oxide. Keep it sealed and bone dry.

Step 4: Reduce with magnesium — the Kroll reactor

mild-steel retort sealed, full of argon titanium sponge grows on wall and floor molten magnesium 800–900 °C magnesium chloride heavier, sinks furnace argon in argon out TiCl₄ feed dripped slowly; rate keeps the heat at 800–900 °C thermocouple well TiCl₄ drops react on the magnesium: TiCl₄ + 2 Mg → Ti + 2 MgCl₂ tap MgCl₂ to the magnesium cell
Fig. 3 The Kroll reactor in cross-section. A sealed mild-steel retort, filled with argon, sits in a furnace. Liquid titanium tetrachloride drips slowly onto molten magnesium; titanium sponge grows on the walls and floor, and the heavier molten magnesium chloride is tapped off from the bottom.
  1. The retort is a closed mild-steel cylinder (a small one: 20–30 cm across, 60–100 cm tall) with a bolted lid carrying a TiCl₄ feed pipe, an argon inlet and outlet, and a thermocouple well (Thermocouples and Thermoelectricity). A tap pipe leaves the bottom. It sits inside a furnace.
  2. Load it with clean magnesium blocks — about 0.3 kg per kg of TiCl₄ you will feed (that is about 20% more than the reaction strictly needs). Bolt it shut.
  3. Pump out the air and fill with argon, three times (The Vacuum Pump). Keep a slight argon pressure on it from now on, so any leak blows out, not in.
  4. Heat to about 800 °C (cherry red). The magnesium melts.
  5. Drip in TiCl₄ slowly. The reaction gives off heat: feed only as fast as keeps the retort at 800–900 °C, opening the furnace or blowing air round the outside if it climbs. A small retort takes most of a day.
  6. Every hour or two, tap the molten magnesium chloride from the bottom into iron pans. It goes straight back to the magnesium cell (Magnesium).
  7. When the magnesium is nearly used up, stop, and let the retort cool under argon. Inside is a crusty grey cake: titanium sponge, soaked with leftover magnesium and its chloride.

Each kilogram of titanium needs about 4 kg of TiCl₄ and 1 kg of magnesium, and gives about 4 kg of magnesium chloride.

Step 5: Clean and melt the sponge

  • Vacuum distillation: heat the cake in the sealed retort to about 1,000 °C under vacuum for a day or more. The magnesium and its chloride boil off and condense in a cooled pipe, leaving clean sponge. (Older plants leached it out with dilute Hydrochloric Acid instead; this leaves more oxygen in the metal.)
  • Melting: press the sponge into a bar, weld bars together under argon to make an electrode, and melt it by an arc onto a water-cooled copper crucible in a vacuum or argon (The Electric Arc Furnace). Melt twice for even metal. A small-scale alternative is a "button" furnace: a sealed chamber full of argon with a pointed tungsten or carbon electrode and a water-cooled copper hearth, melting a few tens of grams at a time.

A sodium-based route (the Hunter process, 1910) works the same way with molten sodium instead of magnesium.

Using titanium

  • Working it. Commercially pure titanium forges at a bright red heat, but scale and absorbed oxygen form a hard, brittle skin that must be ground or pickled off. It work-hardens and conducts heat poorly, so it machines like tough stainless steel: slow speeds, sharp tools, heavy feed and plenty of coolant (Machine Tools). Never let titanium rub on titanium in a bearing — it seizes.
  • Welding. Only under argon, front and back of the weld, until the metal cools below about 400 °C (Welding). The colour tells you the quality: bright silver is good, light straw is acceptable, blue, purple or grey-white flaky means oxygen got in and the weld is brittle.
  • Anodising. Make titanium the positive pole in a bath of washing-soda solution (Soda Ash and Baking Soda) with any metal as the negative, and raise the voltage: a thin oxide grows whose thickness gives colour by interference, as on a soap bubble — roughly bronze at 10–15 V, purple about 20 V, blue 25–30 V, gold about 55–60 V, rose and violet at 65–80 V, and green at about 85–100 V. This is how titanium jewellery is coloured, and colour-coding for implants; Anodising Aluminium and Titanium gives the full method.

How to tell it worked

  • Titanium white: brilliant white when cold, turns pale yellow when red-hot and white again when cool. It does not dissolve in vinegar or dilute acid, and does not blacken in the smoke of burning sulfur or rotten eggs (lead white does). Ground in oil, a thin coat hides black lines.
  • TiCl₄: colourless, boils at 136 °C, smokes in air.
  • Titanium metal: silvery grey, about 60% of the weight of the same piece of steel, not magnetic, gives brilliant white sparks on a grindstone. A strip of good metal bends double cold without cracking; brittle metal snaps.

Note When it goes wrong. Digestion cake stays wet and slushy → acid too weak or ore too coarse; grind finer and use stronger acid. Titanium white comes out yellow or buff → iron left in. Reduce more thoroughly with scrap iron, wash longer, check with gall infusion. White powder comes down while leaching → water too warm; keep it cool, and add the hot liquid to boiling water only at the precipitation step. Sponge brittle and dark → air or water got into the retort, or TiCl₄ was damp. Check every seal and keep argon flowing.

Dangers

Danger Chlorine and TiCl₄. Chlorine gas destroys the lungs (Chlorine and Bleach). TiCl₄ fumes are hydrochloric acid mist; a spill makes a choking white cloud. Do all chlorination outdoors or under a tall flue, upwind, with water and lime ready to neutralise spills. Carbon monoxide from the chlorinator kills silently.

Danger Titanium and magnesium fires. Molten magnesium, fine titanium sponge, powder and machining chips burn with a white heat that water makes worse — water splits into hydrogen and feeds the fire (Magnesium). Keep dry sand or dry salt ready. Never let water or damp material touch the inside of a hot Kroll retort: it can explode.

Danger Hot sulfuric acid. The digestion step boils up suddenly and spits concentrated acid. Wear thick clothing and cover your eyes; stand back after adding the water; work outdoors (Sulfuric Acid, Acids, Bases and Testing).

  • Argon does not poison, but it collects in low places and drowns you without warning: never climb into a pit, tank or furnace where argon may have pooled.
  • Anodising at 50–100 V DC can give a dangerous shock; keep hands dry and use insulated clips (Wiring and Electrical Safety).

What this unlocks

Titanium white makes safe, durable white paint, bright paper, white enamel and glazes. Titanium metal and its alloys build light airframes and jet engines (Gliders and Aeroplanes), corrosion-proof chemical plant and seawater pipes, and bone implants (Crutches, Prosthetics and Rehabilitation, Basic Surgery). Titanium powder is a getter in The Vacuum Tube making, and titanium dioxide is the base of the hard rutile gem made by flame fusion (Synthetic Gems).

How it was first done

In 1791 William Gregor, a Cornish vicar, found a new element in black magnetic sand from a stream in the Manaccan valley. In 1795 the Berlin chemist Martin Heinrich Klaproth found it in rutile and named it after the Titans of Greek myth. For over a century nobody could make the pure metal. In 1910 Matthew Hunter, at Rensselaer Polytechnic Institute in New York, made nearly pure titanium by heating TiCl₄ with sodium in a sealed steel bomb.

Titanium white came first commercially: the sulfate process was brought into production about 1916–1919 by the Titan company at Fredrikstad in Norway and by the Titanium Pigment Company at Niagara Falls in the United States. It soon displaced lead white. DuPont introduced the chloride route, burning TiCl₄ in oxygen, in the 1950s.

William Justin Kroll, a Luxembourg metallurgist, worked out reduction by magnesium under argon in the 1930s and published it in 1940. He moved to the United States, where the US Bureau of Mines scaled it up during and after the Second World War, and DuPont began commercial production of titanium sponge in 1948. Within a decade titanium was flying in jet engines and airframes.

Source: content/entries/metals/titanium.md