Part 5 · Cloth and Clothing
Ropewalks and Sailcloth
How to make long, strong, even rope by the hundred metres on a ropewalk — spinning yarns, twisting strands and laying them with a jack, a top and a sledge — and how to tar it, splice it and test it. Then how to weave heavy hemp canvas and sew it into sails, tarpaulins and tents.
- Difficulty
- ●●●●●
- Time
- A day to build a simple rope machine; an afternoon for 30 m of rope. Weeks to weave a sail's worth of canvas; days to sew it
- Steps from zero
- 7 prerequisites →
This unlocks
Wire Rope and CableTents, Sleeping Bags and Camping GearKites and ParachutesLife Jackets, Lifebuoys and LifeboatsThe full path from nothing — 7 steps before this one
- Cordage and Rope
- Stone Tools
- Basic Woodworking
- Farming from Seed
- Spinning and Weaving Cloth
- Flax, Hemp and Linen
- The Loom
- Ropewalks and Sailcloth
Do them roughly in this order. See it on the tech tree →
Why it matters
Hand-twisted Cordage and Rope is fine for a bowstring or a bundle. But a community soon needs rope by the hundred metres, all of it the same thickness and strength: well ropes and bucket ropes (Wells and Cisterns), hauling and lifting ropes for Cranes and Lifting and building, plough traces and harness (Draft Animals and Harness), rope beds (Furniture), fishing nets and lines (Fishing), bridge cables (Roads and Bridges), the drive ropes of mills (Belts, Chains and Power Transmission), and above all the rigging and anchor cables of ships (Boats and Sails). The ropewalk — a long straight lane where yarns are stretched out and twisted together by a crank — turns rope-making from hours per metre into hundreds of metres per day.
The same fibres, woven heavy and tight, make canvas: sailcloth, tents, tarpaulins, sacks, wagon covers, hammocks, fire buckets and drive belts. The word canvas comes, through French, from cannabis — hemp.
How it works
Rope holds together by twist against twist. Fibres are short; twisting them into a yarn makes them grip each other by friction, so that the yarn breaks only when fibres themselves break. But a twisted yarn wants to untwist. The trick of all rope is to twist each stage the opposite way to the one before:
- Fibres are spun into yarns, twisted right-handed (a Z twist — the slope of the fibres matches the middle stroke of the letter Z).
- Several yarns are twisted together left-handed (S) into a strand. This tightens no yarn and loosens none — it locks them.
- Three strands are twisted together right-handed (Z) into a rope. Each strand, trying to untwist, actually tightens the rope round it.
A rope made like this — three strands, right-handed — is called hawser-laid or plain-laid, and is the standard rope of the world. Three such ropes twisted together left-handed make a cable (cable-laid), very strong and springy, used for anchors.
Twisting shortens everything: a finished rope is only about two-thirds to three-quarters the length of the yarns it was made from. That is why the ropewalk must be longer than the rope you want.
What you need
| Item | Size | Notes |
|---|---|---|
| Fibre | About 100 g per metre of 12 mm rope; 280 g per metre of 20 mm | Hemp is best; flax, nettle, inner bark of lime (basswood) or coir also work (Flax, Hemp and Linen) |
| A straight lane | 1.5 × the length of rope you want | Level, sheltered from wind; a barn, a path along a wall, a field edge. Historic ropewalks were 300–400 m long |
| The jack | Frame 60 × 40 cm | Three cranked hooks turned together. Hardwood with iron hooks, or all-wood hooks |
| The sledge | 60 × 40 cm plank on runners | Carries a single swivel hook and 20–50 kg of stones |
| The top | Hardwood cone or pear shape, 12–20 cm long | Three grooves along it, one for each strand; a handle |
| Stake heads | Posts 1 m high every 5–6 m | T-shaped, with pegs to keep the yarns apart and off the ground |
| Extras | Pine tar (Tar, Pitch and Glue); a strong floor The Loom; sail needles, palm, fid, waxed twine | For tarring, canvas and sails |
Where to find it
- Hemp for rope must be long, strong and well retted (Flax, Hemp and Linen). Long "line" fibre makes the best rope yarn; shorter tow is fine for the cores of strands and for cheap rope.
- Coir — coconut husk fibre — makes rope that floats and resists rotting in seawater, though it is weaker than hemp. Soak the husks for months in a pool or in the sea, then beat out the fibre.
- Other fibres: abacá (Manila hemp), sisal and agave leaves in dry lands, jute, lime and willow bark (Cordage and Rope).
- Wood for the jack, sledge and top: any hard, tough wood — oak, ash, elm, hornbeam, apple. The top must be smooth so the strands slide in its grooves.
Method 1: Spinning rope yarn
Rope yarn is thicker and harder-twisted than yarn for cloth — about 2.5–3 mm thick, like a thick string.
- Hackle the hemp (Flax, Hemp and Linen) and wrap a bundle loosely round your waist, the fibre ends hanging behind you.
- Fix a hook on a turning wheel or on a hand crank at the head of the walk. On a traditional spinning wheel for rope, a big wheel 1–1.5 m across turned by a helper drives several small hooks ("whirls") by a band, so several spinners can work at once.
- Hook a loop of fibre from your bundle onto the turning hook and walk backwards down the walk, letting fibre feed from the bundle through your fingers as the twist runs up to them. A leather pad in your palm protects your hand. Draw out more fibre where the yarn is thin, less where it is thick.
- Lay the yarn on the pegs of the stake heads as you go, so it does not touch the ground.
- At the end of the walk, a helper winds the yarn onto a reel while you walk back. A drop spindle or The Spinning Wheel also works; the walk is simply faster.
Method 2: Making rope on the ropewalk
Build the jack and sledge
- The jack: a stout upright board, 60 cm wide and 40 cm high, braced or staked firmly into the ground. Bore three holes 2.5 cm across in a triangle about 15 cm apart.
- Hooks: three iron rods (or hardwood rods with a hooked fork at the end) passing through the holes. On the back of the board, each is bent into a crank — a Z-shaped bend about 8 cm across — and all three cranks pass through matching holes in a second, loose board, the crank plate. Turning one handle on the crank plate swings the plate round in a small circle and turns all three hooks at the same speed in the same direction.
- The sledge: a heavy plank on two runners, with one hook in a swivel on its front — an iron hook whose shank turns freely in a hole, with a collar to keep it in, and a handle so it can also be turned by hand. Load the sledge with 20–50 kg of stones; more for thick rope.
Make the rope
This method makes a three-strand rope with three people: one at the jack, one at the sledge, one with the top.
- Plan the size. For a 12 mm rope, each strand needs about 5–6 yarns of 2.5 mm; for a 20 mm rope, about 15–17. Scale by the square of the thickness: twice as thick needs four times as many yarns. Twist a short test piece first and measure it.
- Warp the strands. Tie one end of the yarn to the first jack hook, run it down the walk to the sledge hook, back to the same jack hook, and so on, until that strand has its number of yarns. Repeat for the other two jack hooks. Keep every yarn at the same tension; a slack yarn carries no load until the others have broken.
- Tension: drag the sledge back until the yarns are taut and just clear of the stake heads between.
- Form the strands. The jack-turner cranks so that each hook twists its strand against the twist of the yarns — if the yarns are Z, turn so the strands become S. The sledge hook is held still. As the strands twist, they shorten and drag the heavy sledge slowly towards the jack. Twist until each strand is hard: it has shortened by roughly a tenth, and when you slack it a little it tries to curl into a loop.
- Set the top. At the sledge end, set the top between the three strands, each strand in its own groove, with the point of the top towards the sledge. The three strands meet just beyond the top, on the sledge hook.
- Lay the rope. Now:
- the jack-turner keeps cranking the same way, to keep the strands hard;
- the sledge-hand turns the sledge hook the opposite way (or, on a light rope, simply lets it swivel freely);
- the top-man walks the top slowly towards the jack, holding it back slightly. Behind the top, the three strands wind round each other into rope. Walk at a steady pace so the twist is even. A well-laid rope has the strands making one full turn round the rope in a length of about three times its thickness.
- At the jack, take the strands off the hooks, tie them together, and whip both ends (below).
- Finish. Leave the rope stretched under the sledge's weight overnight, then rub it down hard with a pad of old canvas or a handful of tow to lay down loose hairs. Coil it right-handed (clockwise) and hang it in a dry place.
Tarred rope
Hemp left wet rots in a season. Tarring keeps it sound for years in water and weather.
- Heat a pot of pine tar (Tar, Pitch and Glue) until it runs thin like honey — around 100 °C; it should smoke slightly, never boil or flame. Outdoors, with a lid ready.
- Draw the yarns (before laying) slowly through the hot tar, then through a hole in a board lined with a tight ring of tow or leather, which wipes off the surplus.
- Hang the tarred yarns to set for a day, then make the rope as before.
Tarred rope is stiffer and somewhat weaker than untarred rope (by perhaps a fifth), but lasts many times longer. Sailors tarred standing rigging (ropes that never run through pulleys) and anchor cables, and left running rigging untarred so it stayed supple.
Ending and joining rope
Whipping stops an end unravelling. Lay a loop of waxed twine along the rope's end, wrap the twine tightly round the rope and the loop for a length equal to the rope's thickness and a half, push the working end through the loop, and pull the loop's tail to drag it under the wraps. Cut both ends short.
The eye splice makes a permanent loop, and keeps 85–90 % of the rope's strength (a knot keeps only about half; see Knots, Lashings and Rigging).
- Unlay the end for about 12 times the rope's thickness. Whip or tape each strand end.
- Bend the rope into a loop of the size you want. Open the rope's lay with a fid — a tapered spike of hardwood or bone 20–30 cm long.
- Tuck the middle strand under one strand of the rope, against the lay (crossing the rope's strands, not following them).
- Tuck the left strand under the strand next to it, going in where the first came out.
- Turn the eye over and tuck the third strand under the last free strand.
- Now take each strand in turn over one, under one, against the lay, for at least four full rounds. Pull each tight and roll the splice underfoot.
The short splice joins two rope ends the same way: unlay both, push them together so the strands interleave, and tuck each set of strands into the other rope, four rounds each.
Method 3: Weaving canvas
Canvas is plain weave, made as dense as you can beat it. It needs a strong floor The Loom — a light frame loom racks and bends.
- Yarn. Hard-spun hemp or flax. The warp is best two-ply, about 1–1.5 mm thick; the weft can be single and as thick or a little thicker.
- Size the warp. Boil flour or starch with water into a thin paste (about 50 g flour to a litre), soak the warp in it, wring it, and dry it under tension. The size glues down loose fibres so the warp does not fray as the heddles and reed rub it. It washes out later.
- Sett. With 1–1.5 mm yarn, about 10–12 threads per centimetre in both warp and weft. Use a reed with 5–6 dents per centimetre, two threads per dent.
- Width. Historic sailcloth was woven in bolts about 60 cm wide; narrow cloths are easier to beat evenly and are sewn together anyway.
- Beat hard. Make the beater heavy, or bolt a hardwood bar or a strip of iron along its bottom. Beat each pick twice: once in the open shed, once after changing the shed. Aim for as many weft threads per centimetre as warp.
- Weight. Good sailcloth for a small boat weighs about 300–400 g per square metre; for a ship's main sails 500–700 g. Cut a 10 cm square from a sample and weigh it: 3–4 g means 300–400 g/m² (see Measurement from Scratch).
- Shrink it. Wet the finished canvas thoroughly and dry it in the sun before you cut it, so it does not shrink in the sail.
Is it good? Hold it up to the sun: you should see no pinholes of light, only a faint glow. Press your lips to it and blow: it should hardly let any air through. Wetted, it should drip but not stream.
Making a sail
The plan of a working sail — panels, seams, hems, bolt rope, corner patches and reef points — is in Boats and Sails. Here is how the sailmaker does the work.
Tools
- Sail needles: steel needles 6–12 cm long with a three-sided blade behind the point, which parts the threads of heavy canvas instead of pushing them aside (Sewing, Needles and Thread, Iron and Brass Wire).
- The palm: a band of thick leather round the hand, leaving the thumb free, with a hard pad set in the palm — dimpled iron, bone or horn — to push the needle. Without one you cannot get a needle through four layers of canvas.
- Twine: hemp or flax, three to five ply, hard-twisted, drawn over a lump of beeswax so it slides and resists rot.
- A fid for opening holes, a seam rubber (a smooth piece of bone or hardwood) for creasing folds sharp, and a bench hook — a hook on a cord tied to your bench — to hold the work taut while you sew.
Steps
- Lay out the sail full size on a clean floor or flat ground: drive pegs at the corners and stretch cord between them.
- Lay the cloths parallel to the leech (the back edge), each overlapping the last by 3–4 cm. Mark the overlaps and cut each cloth to the outline plus 8–10 cm for the hem.
- Seam. Sew each overlap with two rows of flat stitches, one along each edge of the overlap, stitches about 5–8 mm apart, pulling each one firm.
- Tabling. Fold every edge over twice to make a hem 5–8 cm wide, crease it with the seam rubber, and sew both of its edges.
- Corner patches. Sew two or three extra layers of canvas, cut in triangles or fans 30–60 cm long, onto each corner.
- Bolt rope. Sew a soft, untarred rope all round the edge, about 10 mm thick on a small boat sail, with a stitch through the canvas and between the strands at every lay of the rope. Keep the canvas very slightly slack along the rope so that the rope, not the cloth, takes the strain.
- Grommets and cringles. At each corner and along the top for lashings, make a grommet: a ring laid up from a single rope strand wound three times round itself, sewn into a hole cut in the canvas with close, radiating stitches, then opened round with the fid. A cringle is a similar rope ring worked into the bolt rope itself, standing out from the edge.
- Reef points: short ties of cord sewn through the sail in a row, a hand-span apart.
- Dress it. Working sails were tanned ("barked"): boiled for an hour or two in a strong brew of oak or other tanning bark (Hides and Leather) with red ochre and a little fat or fish oil, then dried. The brown-red sails of fishing fleets came from this. It slows rot greatly.
Tents and tarpaulins
- Tents use lighter canvas, about 250–350 g/m², sewn the same way, with grommets for guy ropes and pegs (Shelter, Tents, Sleeping Bags and Camping Gear).
- Close-woven canvas is showerproof on its own, because the fibres swell when wet and close the gaps. Never touch the inside of a wet tent: your finger wicks water straight through the cloth, and it will drip there all night.
- Tarpaulins were originally canvas coated with tar. Canvas painted with two or three thin coats of boiled linseed oil (Oils and Pressing), each dried for days in the air, becomes oilcloth — fully waterproof, for covers, capes and wagon tilts (Linoleum, Oilcloth and Floorcloths, Raincoats, Oilskins, Umbrellas and Rubber Boots).
How to tell it worked
- Rope: even thickness along its whole length; strands lying snug with no gaps; it does not kink or untwist when hung free. Untwist a short section: the inside should be clean, with no powdery or broken fibres.
- Strength: test a 1 m piece by hanging weight from it. Good hemp rope breaks at roughly 6 × (diameter in mm)² kilograms: about 850 kg for 12 mm, 2,400 kg for 20 mm. That is the low end of commercial hemp ropes; your own first ropes may be weaker, so break test pieces of each batch rather than trusting the formula. Use it at no more than one-sixth of that — about 140 kg for 12 mm — and at one-tenth when lifting people.
- Canvas: no pinholes against the sun, nearly airtight to the breath, weighs what you meant.
- Sail: sets smoothly without hard wrinkles running into the corners.
Note Troubleshooting. Rope is lumpy or uneven → the top was walked unevenly, or the yarns had unequal tension; warp more carefully and keep a steady pace. Rope kinks and won't hang straight → too much twist in the strands for the amount of lay; form them a little less, or lay a little harder. Strands come apart under load → too little twist at the laying stage (a "slack-laid" rope); turn the sledge hook more. Canvas lets light through → too few threads or too light a beat; use a heavier beater and a closer reed. Sail wrinkles at the corners → the bolt rope was sewn too tight or too slack; re-rope that edge.
Dangers
Danger A breaking rope snaps back like a whip. A rope under heavy load stores energy; when it parts, the ends fly back faster than you can move and can break bones, blind or kill. Never stand in line with a rope under strain, or inside a loop (bight) of it. Use ropes at a sixth of their breaking strength, a tenth for lifting people, and throw away any rope that is rotten inside, cut, chafed half through, burnt or stiff with chemicals.
- Hemp and flax dust. Years of breathing the dust from hackling and spinning hemp, flax or cotton cause byssinosis: tight chest, cough and breathlessness, worst at the start of each working week, leading to lasting lung damage. Work dusty jobs outdoors or in a through-draught, damp the fibre slightly, and wear a cloth over your nose and mouth.
- The jack kicks. If a strand breaks while the strands are hard, the handle spins back violently. Grip firmly, stand to one side, and keep children off the walk.
- Hot tar burns, sticks to skin and catches fire. See Tar, Pitch and Glue.
Warning Oily rags and oiled canvas can catch fire by themselves. Cloth soaked in linseed oil heats up as the oil dries; folded or piled, it can smoulder and burst into flame hours later. Hang oiled cloth and rags spread out in the open air until fully dry, or drown them in water.
What this unlocks
Long, strong, uniform rope makes possible Cranes and Lifting and block-and-tackle (Simple Machines), deep Wells and Cisterns, large sailing ships (Boats and Sails, Navigation), suspension and rope bridges (Roads and Bridges), rope drives for mills (Belts, Chains and Power Transmission), rope beds and sprung furniture (Furniture, Mattresses and Upholstery). Canvas makes tents, sacks for Granaries and Food Storage, belting, hoses for Firefighting, and the fabric of the first Balloonss and Gliders and Aeroplanes. When you can draw iron into wire (Iron and Brass Wire), the same ropewalk makes wire rope (Wire Rope and Cable), the cable of mine hoists, suspension bridges and elevators.
How it was first done
Twisted cord is at least 40,000 years old (a three-ply fragment from Abri du Maras in France), and ancient Egyptian tomb paintings, such as that of the official Rekhmire at Thebes (about 1450 BC), show workers making rope. Hemp became Europe's rope and sail fibre in the Middle Ages, and long covered ropewalks were built at every naval dockyard; the double ropery at Chatham in England, finished in 1790, is about 346 m long and still makes rope today. A large sailing warship such as HMS Victory is often said to have carried around 40 km of rope. In the 1790s Joseph Huddart patented machines that gave every yarn in a strand equal tension, making rope much stronger, and by the mid-1800s ropewalks were powered by steam.
Source: content/entries/textiles/ropemaking-and-sailcloth.md