◆ Rebuild

Part 3 · Metals

Forge Shops and Heat Treatment

How a forge shop turns bar into bolts, rivets and forged parts by the thousand with upsetters and heading machines, and how it hardens, tempers, anneals and case-hardens them to a written schedule in proper furnaces and quench tanks, then proves the result with a hardness tester instead of a file and a guess.

Difficulty
●●●●●
Time
A week to build a heading clamp and a gas-fired heat-treatment furnace; one to three months for a power upsetter or a lever hardness tester; a schedule is learned over a season of logged batches
Steps from zero
29 prerequisites →

You need first

Anvils, Trip Hammers and Power HammersAlloy and Stainless Steels

This unlocks

—
The full path from nothing — 29 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. The Kiln
  10. Pottery
  11. Hides and Leather
  12. Bricks
  13. The Wheel and Axle
  14. Firebrick and Refractories
  15. Bellows
  16. Gears
  17. Iron (the Bloomery)
  18. Copper Smelting
  19. The Waterwheel
  20. Blacksmithing
  21. The Blast Furnace and Cast Iron
  22. Magnets
  23. Anvils, Trip Hammers and Power Hammers
  24. Steel
  25. Copper Wire
  26. Steel in Quantity
  27. The Generator
  28. The Electric Arc Furnace
  29. Alloy and Stainless Steels
  30. Forge Shops and Heat Treatment

Do them roughly in this order. See it on the tech tree →

Why it matters

A smith forges one good bolt in ten minutes (Blacksmithing, The Blacksmith's Tooling). A railway or a steam engine needs tens of thousands, all the same and all equally strong. Two things make that possible: upsetting machines that gather a bar into a head in one or two strokes, and heat treatment done by clock and thermometer, not by eye — furnaces that hold an exact heat, quench tanks that cool the same way every time, and a hardness tester that gives a number you can write down.

Steel teaches hardening and tempering by colour, one tool at a time. This is the factory version of the same physics. It feeds Screws, Nuts and Bolts, Nails, Rivets and Wire Fasteners, Springs, Gears, Railways, Boilers and Pressure Vessels and Machine Tools.

How it works

Upsetting. Hitting a hot bar on its end makes it shorter and fatter. The danger is buckling: a long thin end bends sideways instead of swelling. The rule every forge shop uses:

A bar can be upset in one blow if the length left unsupported is no more than 3 times its diameter.

To gather more, upset in several passes, each in a die cavity that stops the metal bending. A bolt head 1.5 diameters across and 0.7 thick needs about 2–2.5 diameters of bar, within the rule, so most bolts take one or two blows.

Heat treatment is a set of recipes for the same steel:

Treatment What you do What you get
Annealing Heat just above the hardening heat, soak, cool as slowly as possible in the furnace Softest state: easy to cut, bend and draw
Normalising Heat 30–50 °C above the hardening heat, cool in still air Fine, even grain; relieves forging strain
Hardening Heat to the hardening heat, soak, quench Hardest, most brittle state
Tempering Reheat hardened steel to 150–650 °C, hold, cool Trades hardness for toughness, exactly as much as you choose
Case hardening Soak low-carbon steel in carbon, then harden Glass-hard skin over a tough core

Temperature decides what happens; soak time decides whether it has happened all the way through. Shop rule: once the surface is at heat, soak 20–30 minutes per 25 mm of thickness for hardening and one hour per 25 mm for annealing and tempering.

What you need

The upsetter

The heading clamp: the simplest version

Build a heading clamp on a heavy bench by the forge: two steel blocks, each with a half-round groove the size of the bar, cut crosswise like a file so the bar cannot slip, squeezed together by a foot lever of 6:1 or 8:1. A stop at the back sets how much bar sticks out.

Heat 2–2.5 diameters of the bar end to bright yellow (1,150–1,200 °C), drop it in against the stop, stand on the lever, and strike the end square with a 2–3 kg hammer until it swells; finish with a heading tool or cupped snap (The Blacksmith's Tooling). Two people head 60–100 bolts an hour this way, against 6–10 by hand.

The power upsetter

Horizontal upsetter, seen from above Crank connecting rod Heading slide 40–80 strokes a minute stock stop heading tool Fixed gripping die grooves for each pass Moving die closes before the blow Cam or toggle on the crankshaft Bar end heated to 1,150–1,200 °C Making a bolt head, in section 1. Gripped 2–2.5 d 2. Gathered 3. Headed 4. Trimmed, rolled hexagon head first punch finishing punch rolled thread
Fig. 1 The horizontal upsetter seen from above. A crankshaft drives the heading slide forward; a cam closes the moving gripping die against the fixed one, clamping the hot bar. Each die block has several grooves, one for each pass. Below, a bolt head in section: gripped, gathered by the first punch, headed by the finishing punch, then trimmed to a hexagon and thread-rolled.

The upsetter (horizontal forging machine) is the heading clamp made automatic and many times stronger.

  • Frame: one heavy cast-iron or cast-steel bed, 3–5 tonnes for bar up to 25 mm, because blow and grip try to tear it apart.
  • Heading slide: driven by a crankshaft and a flywheel of 600–1,200 kg at 40–80 strokes a minute, through a pedal-tripped clutch. It carries the heading tool, a punch with the head shape in its end.
  • Gripping dies: a fixed block and a moving one, closed by a cam or toggle on the crankshaft, timed to grip before the blow and release after. Each block has two to four grooves, from gathering to finishing.
  • Stock stop: a swinging gauge that sets the length sticking out, then swings clear.

Sizes. A 25 mm machine (rated by the largest bar it grips) heads bolts to M24 and needs 7–10 kW; a 50 mm machine needs 20–30 kW and weighs 10–15 tonnes. The grip must at least equal the heading force, or the bar slides back.

Running it. Heat 15–20 bar ends at once in a slot forge. Lay a bar in the first groove against the stop and trip: grip, blow, release. Move it to the next groove and trip again; two or three blows finish a head. Shear the bolt to length hot.

Good versus bad. A good head is solid, square to the shank, with no ring-shaped seam underneath. A cold shut (a fold lapped over and not welded) means too much bar gathered at once, or too cold. Saw a sample head in half and etch it in hot dilute Hydrochloric Acid: the flow lines of the grain should bend smoothly into the head like water round a stone. That flow is why a forged head is stronger than one machined from thick bar.

The bolt header: cold heading

Bolts and rivets below about 20 mm are headed cold from coiled wire on a bolt header, a smaller, faster machine of 60–150 strokes a minute.

  1. Feed rolls push annealed wire (Iron and Brass Wire) forward against a stop.
  2. A cut-off knife shears off a blank of the right length and carries it in front of a solid die, a hardened steel block with a hole the size of the shank.
  3. The first punch (the coning punch) pushes the blank into the die and gathers the end into a cone. This first blow is what lets a cold header gather up to about 4.5 diameters without buckling.
  4. A second punch swings into line (a double-stroke header) and flattens the cone into the finished head.
  5. A knock-out pin in the die pushes the blank out.

The wire must be soft: low-carbon steel (0.1–0.2% carbon), copper or brass, spheroidise-annealed (10–20 hours just below 700 °C, slowly cooled). Hard wire splits the heads. Dies are chromium tool steel at 60–62 HRC, or Tungsten and Filament Wire carbide inserts good for a million parts.

Finishing bolts and rivets

  • Hexagon heads: a trimming press shoves the round head through a hexagonal hole in a hardened die, shearing it six-sided (Presses, Punches and Dies).
  • Threads: cut with dies (Screws, Nuts and Bolts) or, better, rolled in one stroke between two flat hardened dies, one fixed and one sliding, with the thread form cut across their faces. The metal is pushed up, not cut away, so the blank is made to the thread's pitch diameter. Rolled threads are stronger.
  • Rivets are headed the same way, but never hardened. Boiler and bridge rivets (16–25 mm) are hot-headed; tin, copper and small steel rivets are cold-headed (Nails, Rivets and Wire Fasteners).
  • Nuts are sheared from hexagon bar, hot-pierced in a press, then tapped.

The heat-treatment furnace

Heat-treatment furnace, in section Insulating brickin a steel case Firebrickhot face Workno flame touches it Channelunder hearth Bafflewall Thermocouple flue door burner Quench tank Hoist water in water out Thermometer stirrer Overflow Lid openon a fusible link oil, 40–80 °C Basketabove a grid Cooling coil drain
Fig. 2 A gas-fired box furnace for heat treatment. Burners fire under a hearth of firebrick tiles and the flame turns up behind a baffle wall, so it never touches the work. A thermocouple reaches into the work zone. Beside it, the quench tank: oil cooled by a water coil, stirred by a paddle, with a basket on a hoist and a lid held open by a fusible link.

A forge fire is uneven: one part of a bar is orange while the other is red. A heat-treatment furnace surrounds the work with gas and walls at one even temperature.

The simplest version

Build a brick box over a forge: firebrick (Firebrick and Refractories), 30 cm wide, 20 cm high and 45 cm deep inside, with a brick door, set over a coal or charcoal fire that heats its floor and sides while no flame gets in. Put the work in a fireclay or iron box inside it (a muffle), with a thermocouple through the back wall. Tended steadily it holds ±20 °C: good enough for batches of springs and small tools.

The production furnace

  1. Chamber: about 60 cm wide, 40 cm high and 90 cm deep inside; 115 mm firebrick backed by 115 mm insulating brick (Electric Kilns and Furnaces) in a steel case.
  2. Burners: two to four gas or oil burners (Natural Gas and Helium, Petroleum and Refining, producer gas from Coal and Coke), 60–100 kW in all, firing into a channel under a hearth of firebrick tiles. The hot gas rises behind a baffle wall, sweeps back over the work and leaves by a flue near the door. No flame touches the work.
  3. Thermocouple in a closed sheath in the work zone, checked weekly against a cone or a test piece. Later it can drive the burner valve itself through a controller (Process Controllers and Control Valves).
  4. Atmosphere: run slightly rich (a little more fuel than the air needs) to cut scaling. For bright work, pack parts in a closed iron box with cast-iron turnings or spent charcoal.
  5. Tempering oven: a separate box for 150–650 °C with a fan, because still air at low heat layers into hot and cold. Electric is easiest (Electric Kettles, Irons, Heaters and Cookers).

Good versus bad. Put test pieces (or three thermocouples) at the front, middle and back of a full hearth. A good furnace holds them within ±10 °C. A cool front means a leaking door; hot work near the burners means a low or cracked baffle.

Baths. For the most even heat on small parts, use a pot of molten lead (340–900 °C, kept under powdered charcoal) for hardening heats, or a half-and-half mix of sodium and potassium nitrate (Saltpeter), which melts at about 220 °C, as a tempering bath from 250 to 550 °C.

Danger Baths kill. Lead fumes poison (Lead): keep lead below 900 °C, covered, under a hood. A nitrate bath is a strong oxidiser: oil, charcoal or a wet part in it can explode or flare, and above about 600 °C it decomposes. Dry every part and keep carbon away from it. Factories once carburised in molten cyanide, which kills in milligrams: do not use it.

The quench tank

The quench causes more failures than anything else here. A bucket heats up after a few parts; a big enough tank holds its temperature all day.

Size. At least 8–10 litres of oil per kilogram of steel quenched at once, and as much for water. A 20 kg basket needs 200 litres or more. Deep beats wide: the hot oil rises off the work.

Making one.

  1. Tank: riveted or welded steel plate 4–6 mm thick (Sheet Metal and Rolling, Welding), about 60 cm across and 90 cm deep for 200 litres, with a drain valve.
  2. Cooling: a coil of pipe inside, with cold water running through, holding the oil at 40–80 °C. Warm oil quenches better than cold, because it is thinner.
  3. Stirring: a paddle, or a pump drawing from the bottom and jetting at the work, to break up the steam blanket round red-hot steel that leaves soft spots.
  4. Basket and hoist: an iron mesh basket on a chain, lowered quickly and fully, over a grid 15 cm above the sludge.
  5. Lid: hinged steel, held open by a fusible link (a strip of solder that melts in a fire) so it slams shut if the oil ignites. A thermometer in the oil.
  6. Overflow: a pipe near the rim to a drum outside, so a big basket cannot push oil onto the floor.

The quenchants, fastest to slowest:

Quenchant Speed Use
Brine (10% salt in water) Fastest, most even Plain high-carbon steel tools; thick sections
Water at 15–30 °C Very fast Plain carbon steel parts of simple shape; case-hardened parts
Plant oil (rapeseed) or mineral quench oil Medium Thin parts, springs, alloy steels, anything that cracks in water
Still air or a fan Slow High-speed and air-hardening steels (Alloy and Stainless Steels)

Rapeseed oil thickens and goes rancid over months; skim and top it up. Add a handful of Soda Ash and Baking Soda per 100 litres of water against rust.

Good versus bad. Quench a 25 mm bar of your standard tool steel and break it. A good tank gives the same depth of hard, fine-grained rim every time. Soft patches mean poor stirring; cracks mean too fast a quenchant for that steel.

Schedules

Write it down. For every batch record the steel, furnace heat, time at heat, quench and its temperature, temper and hardness. After a season the book gives you the schedule for each steel.

Steel Anneal Normalise Harden Quench Temper for
0.4% carbon (shafts, axles, bolts) 840–870 °C 870–900 °C 830–860 °C Water or brine 550–650 °C: tough parts, 25–30 HRC
0.6% carbon, silicon-manganese (springs) 820–840 °C 860–880 °C 850–870 °C Oil 450–500 °C: about 45 HRC
0.8% carbon (hammers, chisels) 760–780 °C 820–840 °C 790–810 °C Water or brine 250–300 °C: 55–58 HRC
1.0% carbon (files, cutters) 750–770 °C 830–850 °C 770–790 °C Brine 160–200 °C: 62–64 HRC
Oil-hardening tool steel (1% carbon, 1% manganese, ½% chromium) 760–780 °C — 800–820 °C Oil 180–250 °C: 58–62 HRC
High-speed steel 870–900 °C — 1,220–1,280 °C Oil or air 550–570 °C, twice (Alloy and Stainless Steels)

Temper colours (Steel, Materials Data Tables) show only the surface after a few minutes; an hour per 25 mm in the oven soaks right through and gives even hardness.

Case hardening

Low-carbon steel cannot harden, but its skin can be given extra carbon. The box method is in Steel; the shop version:

  1. Compound: 6 parts charcoal (2–6 mm grains) to 1 part sodium or barium carbonate by weight, which speeds the carbon in. Reuse it, topping up with a quarter new each time.
  2. Pack parts in steel boxes with 25 mm of compound round each; seal the lid with fireclay.
  3. Hold at 900–930 °C. Case depth grows with the square root of time, counted from when the box is at heat. Pack carburising is slower than gas, and depths vary with the compound, so treat these as a starting point and break a test pin from every batch:
Time at 925 °C Case depth
2 hours about 0.6 mm
4 hours about 0.85 mm
8 hours about 1.2 mm
16 hours about 1.7 mm
  1. Harden: let the box cool, reheat the parts to 780–800 °C and quench in water or brine.
  2. Temper at 150–180 °C for an hour. A file should not touch the case.

Gears, cams, pins and chain rollers are made this way (Gears, Belts, Chains and Power Transmission). Copper plating (Electroplating) or fireclay paste keeps carbon out where you will drill later.

Flame and induction hardening heat only the skin of a medium-carbon part — a gear tooth, a lathe bed, a journal — with an oxy-acetylene torch (Welding) or an induction coil (Electric Kilns and Furnaces) followed closely by a water spray. Nitriding, in outline: steels with aluminium and chromium held 1–3 days at 500–530 °C in Ammonia gas take a hard skin with no quench and almost no warping.

The hardness tester

50 mm 1,000 mm from the pivot Pivot 5 mm steel ball 750 kg on it Sample on a hardened anvil Screw raises the sample Frame must not spring Oil dashpot load on slowly 37.5 kg weight, 20 : 1 lever d The dent, magnified read d to 0.01 mm, two ways HB = 2F ÷ (πD(D − √(D² − d²)))
Fig. 3 A lever Brinell hardness tester. A 20-to-1 lever loads a 5 mm hardened steel ball against the sample; the weight hangs from the long end, and a screw raises the sample to meet the ball. An oil dashpot lets the load on slowly. Right: the dent as seen under a measuring microscope, and the formula that turns its diameter into a Brinell number.

A hardness tester turns "a file just bites it" into a number. It also tells strength: for steel, the tensile strength in megapascals is about 3.4 times the Brinell number.

The simplest version is the file test. Use a new file, the same light pressure every time, on a ground spot clear of scale. The table at the end of this section shows roughly what it tells you.

The Brinell tester

Press a hardened steel ball into the metal with a fixed load and measure the round dent: soft metal, wide dent. The Brinell hardness (HB) is the load in kilograms divided by the dent's curved area in square millimetres:

HB = 2F ÷ (π × D × (D − √(D² − d²)))

where F is the load in kg, D the ball diameter and d the dent diameter, both in mm.

The standard for steel is a 10 mm ball and 3,000 kg; a 5 mm ball with 750 kg (load scaled to the ball diameter squared) gives the same numbers. Example: a 2.00 mm dent gives HB = 1,500 ÷ (3.1416 × 5 × (5 − 4.583)) = 229, a medium-carbon steel bar.

Building a lever tester.

  1. Frame: a stiff C-shaped casting, opening about 15 cm high.
  2. Lever: steel bar 40 × 60 mm on hardened knife-edge pivots. The ball holder hangs 50 mm from the pivot and the weight 1,000 mm away: 20:1, so 37.5 kg gives 750 kg on the ball. Counterbalance the lever's own weight.
  3. Ball: a 5 mm ball from a ball race (Making Ball and Roller Bearings) in a hardened holder. Replace it if ever flattened.
  4. Anvil and screw: a hardened flat anvil on a coarse screw raises the sample until the lever floats level.
  5. Dashpot: a piston in a cylinder of oil on the lever, so the load comes on over 2–3 seconds, not as a blow.

Using it. Grind the spot flat. Let the load on, hold 15 seconds, lift. Measure the dent two ways at right angles with a microscope with a scale (The Microscope, Rules, Squares, Callipers and Gauges) to 0.01 mm, and average. The sample must be at least 10 times as thick as the dent is deep. A steel ball flattens on hard work, so Brinell is good only to about 450 HB (about 47 HRC).

Rockwell and Vickers, in outline

For harder work, use a diamond (Industrial Diamond and Hard Abrasives).

  • Rockwell C: a 120° diamond cone with a rounded tip goes in under a 10 kg minor load; a dial gauge is zeroed; a 150 kg major load is added and removed; each 0.002 mm of extra permanent depth is one point below 100. Read straight off the dial.
  • Vickers: a square diamond pyramid, 136° between faces. HV = 1.854 × F ÷ d², with d the dent's diagonal in mm. Works from the softest metal to the thinnest case.
File test Rockwell C Brinell Typical part
Cuts easily under 20 under 230 Mild steel, annealed tool steel
Cuts with effort 25–35 250–330 Shafts, bolts, tough gears
Bites lightly 45–50 430–480 Springs, hammers
Barely bites 55–58 (use diamond) Chisels, punches
Skates 60–65 (use diamond) Files, knives, case-hardened skins

How to tell it worked

  • Hardness: every part within ±2 HRC (±15 HB) of target; test one from the front, middle and back of each load.
  • Break test: weekly, harden and break a notched bar of each steel. The break should be fine and silky grey; coarse, sparkling grain means overheating.
  • Case depth: break a case-hardened test pin and wipe it with a little nitric acid in alcohol (Nitric Acid); the case shows as a darker ring.
  • Bolts: one bolt per batch pulled in a Strength of Materials lever rig must break in the thread, never under the head.

Note Troubleshooting. Heads split on the cold header → wire too hard or too high in carbon; spheroidise-anneal it, or head it hot. Bent or folded heads in the upsetter → too much bar left out for one pass; use another groove, or upset hotter. Soft spots after quenching → steam blanket; stir harder, use brine, or clean off scale before hardening. Cracked in the quench → too hot, too fast a quenchant, or a sharp corner; harden 20 °C lower, quench in oil, round the corners, and temper within the hour. Hardness varies across a load → uneven furnace; fix the baffle, load less, soak longer. Warped long parts → heat them hanging, quench them vertically, end first.

Dangers

Danger Quench-oil fires. Too much red-hot steel in too little oil boils it and sets the tank alight. Keep the volume up, the lid on its fusible link, dry sand nearby, and never use water on burning oil. Quench under a hood: the smoke chokes.

Danger Machines that crush. An upsetter's dies close with tens of tonnes. Fit a guard and a trip that cannot repeat by itself; use tongs, never hands; lock out the clutch before changing dies.

  • Hot scale and spatter: leather apron, gloves, face shield, boots with no gaps.
  • Carbon monoxide from carburising boxes and rich furnaces: vent the shop high and low.
  • Untempered parts can burst on the bench hours later. Temper the same day.

What this unlocks

Bolts and rivets of known strength let you design Railways, Steel Frames and Tall Buildings, Boilers and Pressure Vessels and Cranes and Lifting by calculation (Strength of Materials). Repeatable hardening gives Springs, Gears, Making Ball and Roller Bearings, cutters for Machine Tools and dies for Presses, Punches and Dies. A hardness number is the first written specification, the root of Precision and Interchangeable Parts.

How it was first done

René Antoine de Réaumur studied case hardening and tempering scientifically in France and published in 1722, grading steels by which minerals scratched them. Bolt- and rivet-heading machines were at work in Britain and the United States by the mid-1800s. Dmitry Chernov in Russia showed in 1868 that steel must pass critical temperatures to harden, turning craft lore into science. The Swede Johan August Brinell showed his ball test at the Paris Exposition of 1900; Hugh and Stanley Rockwell in Connecticut patented their depth-reading tester in the 1910s to check bearing races; Robert Smith and George Sandland at Vickers in England introduced the diamond pyramid in the early 1920s. Adolf Fry in Germany developed nitriding steels around 1921–1923.

Source: content/entries/metals/forging-and-heat-treatment.md