◆ Rebuild

Part 15 · Knowledge and Science

Lenses

How to grind and polish a glass lens by hand with nothing but stone or iron tools, sand and rust — and how to make a tiny glass-bead lens that shows you bacteria. Lenses give you fire from sunlight, spectacles, the microscope and the telescope.

Difficulty
●●●●●
Time
1–3 days of grinding and polishing per lens; an hour for a bead lens
Steps from zero
7 prerequisites →

You need first

Glass

This unlocks

Hearing Aids, Braille and Daily-Living AidsThe Darkroom and the EnlargerMicrofilm and Document StorageThe MicroscopeOptical Glass and Achromatic LensesPhotographySpectaclesThe SpectroscopeThe TelescopeVacuum Coating and Thin FilmsHarbours and Lighthouses
The full path from nothing — 7 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. The Kiln
  4. Pottery
  5. Lime
  6. Lye and Potash
  7. Glass
  8. Lenses

Do them roughly in this order. See it on the tech tree →

Why it matters

A piece of curved glass bends light. That simple fact gives you:

  • Fire from sunlight with no fuel or friction (see Fire).
  • A magnifier to inspect fine work, splinters, seeds, insects and cloth.
  • Spectacles (Spectacles). Almost everyone over 45 slowly loses the ability to focus close up. Reading glasses give craftsmen, scribes and healers another 20 years of fine work.
  • The The Microscope, which shows the living things that cause disease — the foundation of Sanitation and Germs and modern medicine.
  • The The Telescope, for navigation, survey, spotting at a distance, and astronomy.

How it works

Light travels more slowly in glass than in air, so it bends when it enters or leaves glass at a slant. A convex lens — thicker in the middle than at the edges — bends all the light passing through it towards a single point, the focus. The distance from the lens to that point, for light from far away, is the focal length (written f). The more strongly curved the lens, the shorter the focal length and the stronger the lens.

A concave lens — thinner in the middle — spreads light out. It corrects short sight and is used in some telescopes.

Two rules of thumb for ordinary glass:

Lens shape Focal length
Both faces curved, both ground on a tool of radius R f ≈ R
One face curved (radius R), the other flat f ≈ 2R

So to make a lens of a given strength, you choose the radius of the tool. A magnifier with f = 5 cm needs a tool of radius 5 cm (both sides) or 2.5 cm (one side); a reading lens with f = 50 cm needs a gentle curve of radius 50 cm.

Why hand grinding works. If two hard surfaces are rubbed against each other with grit between them, in strokes that keep changing direction, the high spots wear away until the two fit together everywhere. The only shapes that fit each other in every position are a matching ball and socket — a convex and a concave sphere of the same radius. So random rubbing makes perfect spherical curves automatically. This is the secret of all optical work done without machines.

What you need

Item Details
Glass blank Clear, bubble-free Glass disc, 4–6 cm across, 6–10 mm thick; better still, Optical Glass and Achromatic Lenses
Grinding tools Two discs of fine-grained stone, iron, Bronze or brass, a bit larger than the lens: one convex, one concave, of the radius you want
Template A thin board cut to the curve with a string compass
Handle A wooden knob the size of a large cork, and some pitch to stick the lens to it
Abrasives Sharp quartz sand, emery or garnet sand, in several grades; see below and Abrasives and Grinding Stones
Polish Rouge (fine red iron oxide), tin oxide, or very fine wood ash
Polishing lap Pine pitch (see Tar, Pitch and Glue), or felt, leather or paper
Water, jars, rags Lots. Everything must be kept spotlessly clean

Where to find it

  • Sand: clean quartz sand from rivers, dunes and beaches; quartz is harder than glass and cuts it. Sieve it through cloth.
  • Emery: a dark grey to black rock, very heavy for its size, made of corundum (the mineral of rubies and sapphires) mixed with iron oxide. It is harder than quartz and scratches it. Famous deposits are on the Greek island of Naxos and in western Turkey. Garnet sand — dark red to black, heavy grains that collect in streaks on some beaches and in river bends — is a good substitute. So is crushed flint (see Stone Tools).
  • Rouge: heat green vitriol (see Sulfuric Acid) in a clay pot at red heat until it is all a dark red powder (this is colcothar), then wash it many times in water. Or grind red iron ore (hematite) or red ochre clay very fine. Or roast iron rust.
  • Tin oxide ("putty powder"): melt tin in an open dish and keep stirring; skim off the grey-white powder that forms. A historic lens polish.
  • Wood ash: fine, white ash from hardwood fires, sieved and washed.

Step by step

1. Make the blank

Gather a blob of molten glass, drop it onto a smooth, pre-heated stone or clay slab, and press it into a disc about 8 mm thick with a pre-heated flat stone or wet wooden paddle. Anneal it: bury it at once in hot ash, or put it in the cooling end of your glass kiln, so it cools slowly over several hours. Glass cooled quickly is full of strain and cracks when ground. Choose the clearest discs, with no bubbles or streaks in the middle. Round the edge on a flat stone with sand and water.

(Thick pieces of old bottle or window glass work if you have them, but the method above needs nothing salvaged.)

2. Make the tools

  1. Cut a template. Tie a string to a nail, measure R along the string, and scribe an arc on a thin board. Saw along the arc: one piece is a convex template, the other concave.
  2. Rough out two tools. Shape two discs of stone or metal, one bulging (convex) and one hollow (concave), to match the templates. Stone is pecked and ground; metal can be cast in a Finding and Preparing Clay mould (see Metal Casting).
  3. Grind them together. Put a spoonful of wet coarse sand between them. Rub the top one over the bottom one in short, wandering strokes, turning it a little every few strokes and walking slowly around the work. Swap which one is on top now and then. Keep going until a thin line of charcoal drawn across each face is rubbed off evenly everywhere after a few strokes — that means they fit all over. Check against the template; if the curve has drifted, rub with the concave tool on top to deepen it, or the convex tool on top to flatten it.

3. Grind the lens

SECTION SEEN FROM ABOVE short strokes, ⅓ of the lens width Wooden handle Pitchholds the glass Glass blank Wet gritsand → emery → rouge Concave tool stone or iron, ground to radius R walk slowly round the tool turn the lensa little everyfew strokes strokes cross the centre,always changing direction
Fig. 1 Grinding a lens. The glass blank, stuck to a wooden handle with pitch, is rubbed in the concave tool with wet grit. Short strokes in changing directions, turning the lens and walking around the tool, keep the curve spherical.
  1. Mount the blank. Warm the pitch and the wooden handle, press the blank onto it, centred, and let it cool hard.
  2. Coarse grinding. Wet the concave tool and sprinkle on coarse grit. Rub the glass in the tool with short strokes about one third of the lens's width, the lens passing back and forth over the centre of the tool. Change direction constantly, give the handle a small turn every few strokes, and move around the tool. Add grit and water when the grinding sound fades from a gritty crunch to a soft hiss. Continue until the curve reaches the edge of the lens all the way round — perhaps 30–90 minutes.
  3. Finer grades. Wash everything — lens, tool, handle, hands, bench — so not one coarse grain remains. Then grind with the next finer grit for 15–30 minutes. Repeat through four or five grades. At each stage, look at the surface under a strong side light with a magnifier (or the water-drop lens below): grind until all the larger pits left by the previous grade are gone and the surface is an even, fine frosting.
  4. Re-true the tools by grinding them against each other briefly between lenses.

Tip Grading grit by settling. Stir a handful of abrasive powder into a tall jar of water. After 10 seconds, pour the cloudy water into a second jar; what stays behind is coarse. Wait 1 minute and pour again into a third jar: the sediment in the second jar is medium. Repeat after 10 minutes and 1 hour. Each later jar holds finer grit. Ancient and modern lens makers both graded abrasives this way.

4. Polish

  1. Make a pitch lap. Warm the concave tool and pour on a layer of soft melted pitch, 3–5 mm thick. While it is still soft, wet the ground lens with rouge-and-water and press it into the pitch so the pitch takes its exact curve. When cool, cut grooves 2–3 mm wide across it in a grid of squares about 1 cm, so polish and water can flow. The pitch is right when a thumbnail pressed into it for five seconds leaves a shallow dent.
  2. Polish with a thin cream of rouge and water, using the same strokes but light pressure. Polishing is slow: 1–3 hours per side for a small lens. Re-press the lens into the warm lap if it stops touching all over.
  3. Stop when, held in a strong beam of light, the surface shows no grey haze and no pits.

Felt, leather or several layers of paper glued to the tool and charged with rouge also polish well; they are easier but can slightly round the edges.

5. The second side

Remove the lens from the handle by warming the pitch. Mount it the other way up and repeat steps 3 and 4 — on the same tool for an equal biconvex lens, or on a flat stone (ground flat against two other flat stones in turn) for a plano-convex one.

Keep it centred. The lens must be equally thick at every point of its edge, or images will be blurred and coloured. Check by pinching the edge between two sticks at several places round it. If one side is thicker, press harder over that side during coarse grinding.

How to tell it worked

Sunlightparallel rays Lens Card Focal length f from the lens to the smallest, brightest spot LENS SHAPES Two curved facesf ≈ R of the tool One face flatf ≈ 2 × R Concavespreads light;for short sight
Fig. 2 Measuring focal length with the sun. Move the lens until the spot of light on the card is as small and sharp as possible; the distance from lens to card is the focal length. A short focal length means a strong lens.
  • Measure the focal length. Hold the lens in sunlight over a card and move it until the bright spot is smallest and sharpest. The distance from the middle of the lens to the card is f. (Or, indoors, focus the image of a distant window onto a wall.) Spectacle strength is given in dioptres: 100 divided by f in centimetres. A lens with f = 50 cm is +2 dioptres.
  • Look through it. Straight lines of a woven mat or ruled page should look straight and sharp across the middle. Fuzziness everywhere means poor polishing; fuzziness or colour at one side means the lens is off-centre.
  • Hold it in a sunbeam in a dark room. Scratches and pits light up. A few faint ones are tolerable; a haze is not.

Note Troubleshooting. Deep scratches appear during fine grinding → a coarse grain got in. Wash everything and go back one grade. The lens cracked → it was not annealed, or the pitch was too hot when mounting. The edge never gets ground; only the middle → the tool's curve is deeper than the lens; grind longer or re-true the tools. Polishing takes forever → the lap no longer fits; warm it and re-press it.

Using lenses

Use Lens Notes
Burning glass Large (8–15 cm across), f 20–50 cm Focus on charred cloth or dark tinder
Magnifier f 5–10 cm Magnifies about 25 ÷ f (in cm): 2½–5 times
Reading spectacles +1 to +3 dioptres (f 100 to 33 cm) Let the wearer try several and choose; mount in frames of horn, bone, wood or wire
Spectacles for short sight Concave, ground on the convex tool Strength chosen by trial
Simple telescope Objective f 50–100 cm, eyepiece f 2–5 cm Magnification = objective f ÷ eyepiece f. See The Telescope
Compound microscope Two short-focus lenses in a tube See The Microscope

The water-drop and glass-bead microscope

The strongest simple lens is a tiny sphere. You can make one in an hour, without grinding, and it magnifies more than early compound microscopes did.

THE HOLDER SECTION, ENLARGED Bead1–2 mm Needleholds thespecimen two thin plates of copper,brass, horn or wood Eyepressed close Glass beadheld between two holes Specimenabout 1 mm from the bead plates slide to focus Bright skyor a candle — never the sun
Fig. 3 A single-lens bead microscope. A glass bead 1–2 mm across sits in a small hole in a thin plate. The specimen, on a needle or a drop of water, is held almost touching the bead. Hold the plate right against your eye and look at a bright sky through it.

Water drop. Bore a clean hole 3–4 mm across in a thin strip of metal, horn or wood about 1 mm thick. Place a drop of clear water in the hole so it bulges on both sides. Hold it close to your eye and close to a leaf or an insect: you will see it magnified several times — enough to inspect fine work or grind finer lenses.

Glass bead.

  1. Heat a thin rod of clear glass in the hottest part of a flame (an oil lamp blown with a mouth blowpipe, or a small charcoal fire with Bellows) until it softens, then pull the ends apart to draw a thread about 1 mm thick.
  2. Hold the tip of the thread in the flame. It melts and pulls itself into a ball. When the ball is 1–2 mm across, take it out and let it cool. Break the thread off close to the ball.
  3. Make a holder: two thin plates of copper, brass, horn or hard wood, each with a hole slightly smaller than the bead. Sandwich the bead between the holes and pin or rivet the plates together.
  4. Mount a needle or pin in front of the bead, about 1 mm away, that can be screwed or slid closer and further. Put the specimen on its tip: a drop of pond water, a scraping from your teeth, a slice of cork, a mould spore.
  5. Hold the plate against your eye and look towards bright sky or a candle flame behind the specimen. Move the needle until the specimen is sharp. The depth of focus is tiny; be patient.

A 1.5 mm bead magnifies about 150–200 times. In pond water you will see swimming single-celled creatures; with care and good light, even bacteria. This is direct proof that living things too small to see exist everywhere — the heart of Sanitation and Germs.

Dangers

Danger Never look at the sun through a lens or telescope, even for a moment. The focused sunlight burns the retina instantly and permanently. Never let anyone, especially a child, point a lens at the sun near their eyes.

Warning Fumes from roasting green vitriol to make rouge are choking and acid (sulfur oxides) — they damage the lungs. Do it outdoors, downwind, and stand back.

  • Fire. A lens left in sunlight — on a window sill, in a bag, on dry grass — can start a fire hours later. Keep lenses covered.
  • Silica dust. Dry-grinding sand, flint or glass produces dust that scars the lungs over years (silicosis). Always grind wet, and sweep up wet.
  • Glass slivers fly when chipping edges or drawing threads; protect your eyes.
  • Hot pitch sticks to the skin and keeps burning; cool it at once in water.

What this unlocks

With lenses you can build the The Microscope and The Telescope, make spectacles, start Fire from sunlight, and see clearly the fine details of every other craft. A lens and a dark box make a camera obscura, which projects a picture of the world onto a wall — a drawing aid and, much later, the camera (Photography). Lenses that let through more light and less glare come from Optical Glass and Achromatic Lenses and anti-reflection coatings.

How it was first done

A polished rock-crystal lens from about 750–710 BC was found at Nimrud in Iraq; nobody knows whether it was used to magnify. In 423 BC the Greek playwright Aristophanes joked about using a "burning stone" to melt the writing off a wax tablet recording a debt. The Roman Seneca noted that letters look larger through a glass globe of water. Around 1021, the scientist Ibn al-Haytham in Cairo wrote the Book of Optics, explaining how lenses and the eye work. Spectacles were invented in northern Italy around 1286. In 1608 spectacle makers in the Netherlands put two lenses in a tube to make the first telescope, the next year Galileo built his own, and in January 1610 he found the moons of Jupiter. In the 1670s the Dutch cloth merchant Antonie van Leeuwenhoek, using single tiny lenses he ground and melted himself, became the first person to see bacteria and single-celled life.

Source: content/entries/knowledge/lenses.md