Part 15 · Knowledge and Science
Paper
How to turn plant fibre — old linen rags, hemp, flax, mulberry bark or tough grasses — into sheets of paper by cooking it in lye, beating it to pulp and lifting it from water on a screen. Cheap paper is what makes books, records and printing possible.
- Difficulty
- ●●●●●
- Time
- 1–3 days to prepare and cook fibre, half a day to beat it, then about 1 minute per sheet; 1–3 days to dry
- Steps from zero
- 4 prerequisites →
You need first
Lye and PotashThe full path from nothing — 4 steps before this one
Do them roughly in this order. See it on the tech tree →
Why it matters
Clay tablets are heavy, wax smears, bark is small, and parchment needs the skin of an animal for every few pages. Paper is light, cheap, foldable, takes Ink well, and can be made by the thousand from plants and worn-out cloth. Every book is paper. Without it, Printing is pointless — a printing press can use up a whole calf's worth of parchment in a few minutes.
Paper is also useful far beyond writing: wrapping, filters for Distillation and chemistry, lampshades, patterns and templates for Basic Woodworking, cartridges, and oiled paper for windows when you have no Glass.
How it works
Plants are built from long, thin cells made of cellulose — the same stuff as cotton. Paper is simply a mat of these fibres, laid down from water so they cross and tangle in every direction. As the wet mat dries, the fibres pull together and stick to each other by themselves; no glue is needed.
To get there you must:
- Free the fibres from the plant's other material (sticky gums, the woody binding called lignin, starch, bark). Rotting (retting) and cooking in alkaline Lye and Potash dissolve that material and leave the cellulose.
- Beat the fibres so they split, fray and soften. Frayed fibres hug each other and make strong, smooth paper. Un-beaten fibre makes weak, hairy, lumpy sheets.
- Form a sheet by catching the fibres on a fine screen as the water drains through.
- Press and dry it.
- Size it — fill its pores with gelatin or starch — so ink sits on the surface instead of spreading like on a cloth.
What you need
| Item | Details |
|---|---|
| Fibre | About 100 g of dry, cleaned fibre makes 15–25 letter-sized sheets |
| Lye | Weak lye made from wood ash (see Lye and Potash) — enough to cover the fibre |
| Cooking pot | A large Pottery or iron pot (not copper, which stains) |
| Beating stone and mallet | A flat smooth stone or hardwood block; a wooden mallet or club |
| Vat | A tub, trough or large pot that your mould fits into with a hand's width to spare |
| Mould and deckle | Below |
| Felts | Squares of woollen cloth, felt or smooth linen, a little larger than the sheet — one per sheet |
| Press | Two flat boards and heavy stones, or a lever or screw press (see Simple Machines) |
| Size | Hide scraps, bones or hooves for gelatin; or flour or rice for starch |
Where to find it
The best fibres are long, strong and nearly pure cellulose.
- Linen and cotton rags. For 1,800 years most of the world's paper was made from worn-out cloth. The fibres have already been cleaned by spinning, weaving and washing. Use plant-fibre cloth only — wool and silk dissolve in lye.
- Hemp and flax. Tall annual plants with long fibres in the "skin" of the stem (bast fibres). Flax: slender, 60–100 cm tall, small blue flowers, used for linen. Hemp: 1–4 m tall, leaves split into 5–9 narrow saw-edged fingers. Both are grown from seed in one summer; see Spinning and Weaving Cloth.
- Mulberry bark. The inner bark of paper mulberry (Broussonetia) is the classic paper fibre of China, Korea and Japan; true mulberry, fig and other trees with tough, stringy inner bark also work. Cut young shoots in winter, steam or soak them, and peel the bark. Scrape off the dark outer skin; keep the white inner layer.
- Grasses and leaves. Rice and wheat straw, bamboo, cattail and iris leaves, yucca, nettle, daylily, cornhusk and banana stems all make paper — usually weaker and darker than rag. Mix them with a better fibre.
- Not wood, at first. Wood fibre is short and bound by lignin; making good paper from it needs strong chemicals and heavy machinery (Wood Pulp, Kraft Paper and Paperboard).
Step by step
1. Prepare the fibre
- Rags: unpick seams and hems, cut into pieces about 2–3 cm square, and soak in water for a day. Historically, rags were left in damp heaps for several weeks to ferment and soften; this works but smells.
- Hemp and flax stalks: ret them — soak bundles of stalks in a pond or slow stream for 1–3 weeks, until the fibres peel easily from the woody core. Dry, crush the stalks with a wooden mallet, and shake and scrape out the woody bits. Cut the fibre into 2–3 cm lengths.
- Mulberry bark: soak the stripped inner bark overnight.
- Grasses: cut into 2–3 cm lengths.
2. Cook in lye
- Make weak lye from wood ash as described in Lye and Potash: it should feel slippery between finger and thumb, and a fresh egg should sink or barely float in it (strong lye floats an egg high — dilute it).
- Put the fibre in the pot, cover it with lye, and simmer gently: 2–3 hours for grasses and mulberry, 3–6 hours for hemp, flax and rags. Stir now and then and keep it covered with liquid.
- Test: pull a strand. When it separates easily along its length into fine fibres, it is cooked.
- Rinse thoroughly — in a basket in running water, or in many changes of clean water — until the water runs clear and the fibre no longer feels slippery. Left-over lye turns paper yellow and brittle.
3. Beat
- Squeeze a ball of wet fibre and lay it on the stone. Beat with the mallet, folding and turning the mass, for 1–3 hours for each double-handful — longer for rags and hemp, less for mulberry. Keep it wet.
- Test often: drop a pinch into a jar of clear water and shake. Well-beaten fibre spreads into an even cloud of separate fibres, like smoke. Lumps or visible strings mean beat more.
Beating is the hardest work in papermaking. Mills of the past used rows of hammers lifted by a The Waterwheel (stampers) and, from the 1680s, a beater with a bladed roller (the Hollander). A heavy wooden pestle in a stone mortar is the hand version.
4. Make a mould and deckle
- Mould. A rigid frame of straight hardwood strips 2 × 2 cm, with inside dimensions of the sheet you want (start with about 20 × 30 cm). Add 2–4 thin cross-ribs underneath to support the screen.
- Screen. It must drain fast but hold fibres. Options, from best to simplest:
- A laid screen: hundreds of thin, straight, round splints of bamboo, reed or grass stem (1–2 mm thick) laid side by side and stitched together every 2–3 cm with fine thread — the Asian method.
- Woven wire, once you can draw copper or brass wire (Iron and Brass Wire, Copper Wire).
- A tightly stretched piece of fine, even-woven linen or cotton cloth, nailed or tied around the frame.
- Deckle. A second, lighter frame of exactly the same inside size, without a screen, which sits snugly on top of the mould.
Tip The simplest start: the floating mould. Stretch cloth on a frame with no deckle. Float the frame in a shallow pool, pour a measured jug of pulp onto it, spread it with your fingers, and lift it out. Let the sheet dry on the cloth in the sun, then peel it off. You need one frame per sheet per day, but it is very forgiving. Paper is still made this way in Nepal and Thailand.
5. Form the sheets
- Fill the vat with clean water and add pulp until it looks like thin milk with fibres floating in it: about 1 part beaten pulp to 20–30 parts water. Stir well before every sheet; fibre sinks.
- Dip. Hold the mould, screen up, with the deckle on top. Slide it into the far side of the vat at a steep angle, turn it flat under the surface, and lift it straight up, level.
- Shake. As the water pours through, give a quick shake side to side, then front to back. This crosses the fibres so the sheet is equally strong both ways. Stop before the sheet loses its wet shine. The whole dip takes 5–10 seconds.
- Check. Hold it up: the layer should be even, like a smooth blanket. Thin spots, holes or lumps? Tip the mould face down onto the water's surface, the pulp floats off; try again.
- Couch (say "cooch", from the French for "lay down"). Lift off the deckle. Turn the mould upside down onto a damp felt in one smooth rolling motion — one long edge down first, then roll it flat, press firmly, and roll it up off the other edge. The wet sheet stays on the felt.
- Stack. Lay another damp felt on top, couch the next sheet, and so on. A pile of 10 to 100 felts and sheets is called a post.
6. Press and dry
- Put a board on top of the post and press: stand on it, load it with heavy stones, or tighten a press. Water will stream out. Press as hard as you can for 10–30 minutes.
- Peel each sheet carefully off its felt. Either hang 3–5 sheets together over a cord or pole in a shaded, airy place (the old European way), or brush single sheets onto a smooth board or plastered wall to dry flat (the Asian way, which gives one smooth side).
- Dry slowly, out of direct sun and wind, for 1–3 days. Sheets dried too fast curl and cockle.
- Press the dry sheets under boards for a few days to flatten them.
7. Size
Unsized paper ("waterleaf") drinks ink like blotting paper. It is fine for printing with oily ink but not for pen and ink.
- Gelatin size (European): simmer clean scraps of hide (see Hides and Leather), skin, hooves or bones in water for several hours (do not let it boil hard), strain, and you have glue water — see Glues and Adhesives and Gelatin for animal glue. Dilute it until it is just slightly sticky between the fingers when warm and sets to a weak, wobbly jelly when cold, roughly 2–5% gelatin. Keep it warm (about 40–50 °C — hot to the hand but not painful). Dip each dry sheet in, drain, and dry again.
- Starch size (Chinese and Islamic): boil 1 part wheat or rice flour (or pure starch) in 20 parts water to a thin, clear paste. Brush it on both sides, dry, then rub the surface with a smooth stone or shell (burnishing) for a hard, glossy writing surface.
How to tell it worked
- Look through it against the light: fibres should be spread evenly, without clouds, thin patches or lumps.
- Tear it: good paper tears with a fuzzy edge of long fibres and resists. Short, clean tears mean the fibre was over-cooked, under-beaten, or a weak plant.
- Fold it in half, then in half again, along the same line, several times. Good rag paper survives dozens of folds.
- Write on it with Ink: sized paper gives a sharp line; ink that spreads in a fuzzy halo means the size is too weak.
Note Troubleshooting. Sheets stick to the mould → shake less and drain longer; or the screen is too rough. Sheets fall apart when lifted from the felt → too little pulp in the vat, or under-beaten fibre. Add pulp, beat longer. Paper is brown and brittle → lye not rinsed out, or cooked too long in strong lye. Blisters and bubbles after couching → you set the mould down flat instead of rolling it. Paper is stiff and hairy → not beaten enough.
Other writing materials
Papyrus
Where the papyrus sedge grows (tall, triangular green stems with a mop-head of thin stalks, in the shallows of the Nile and other warm rivers and swamps), you can make papyrus, the paper of ancient Egypt:
- Cut fresh stems, peel off the green rind, and slice the white pith lengthwise into strips about 2–3 cm wide and 1–2 mm thick.
- Soak the strips in water for a day or more.
- Lay strips side by side, edges just overlapping, on a cloth. Lay a second layer across them at right angles.
- Cover with cloth and beat gently with a mallet, then press under boards and stones for several days. The plant's own sap glues the layers together.
- Dry, then polish with a smooth stone or shell.
Glue sheets edge to edge with starch paste to make a long roll.
Parchment and vellum
Parchment is animal skin made into a thin, strong writing sheet — not tanned leather.
- Soak a fresh calf, sheep or goat skin in lime water (slaked Lime in water, like thin milk) for 3–10 days, stirring daily, until the hair slips out at a touch.
- Scrape off the hair on one side and the fat and flesh on the other with a blunt, curved blade over a smooth log. Rinse well.
- Lace the wet skin by its edges into a wooden frame with cords, and tighten as it dries.
- While it is damp and stretched, scrape both surfaces thin and even with a sharp crescent-shaped knife. Let it dry under tension.
- Rub with pumice or fine sandstone to finish. Vellum is the finest parchment, from calfskin.
Parchment lasts a thousand years, but one calf skin gives only a few large pages. A full Bible needed the skins of more than a hundred animals.
Dangers
Danger Lye and lime burn skin and blind eyes. Hot lye splashing into an eye can cause permanent blindness within seconds. Wear eye protection of some kind (even a strip of thin cloth or a glass visor is better than nothing), keep clean water close, and if any lye or lime water reaches the eye, hold it open and pour clean water across it, from the nose side outward, for at least 30 minutes (Emergencies). Lye makes skin feel soapy — that is your skin dissolving; rinse at once.
- Boiling pots of lye are heavy and tip easily. Set them on a stable fire base and keep children away.
- Retting and rag fermenting pollute water and stink. Ret downstream of where anyone drinks, and never in a drinking-water pond.
- Cold, wet work for hours chills hands; work in shifts and warm your hands.
- Mould grows on damp pulp and on paper stored damp. Use pulp within a few days or keep it dry; store paper dry and off the floor.
What this unlocks
With paper you can keep cheap records (Writing and Numbers), make books, and — with Ink and a press — Printing. Paper filters help in Distillation and chemistry; paper patterns help with Basic Woodworking and Metal Casting.
How it was first done
Papyrus was made in Egypt by about 3000 BC; the oldest written papyrus rolls found so far, the logbook of an official named Merer, are about 4,500 years old. Parchment spread from the eastern Mediterranean in the last centuries BC — legend credits the city of Pergamon, which gave parchment its name. Paper itself was invented in China: fragments of plant-fibre paper date to the 2nd century BC, and in AD 105 the court official Cai Lun presented an improved method using bark, hemp, rags and old fishing nets. Papermaking reached Samarkand by the 8th century and Baghdad by about 794, and Islamic papermakers perfected rag paper and starch sizing. It reached Spain in the 11th or 12th century. The Italian mills of Fabriano, in the 13th century, introduced water-powered stampers, gelatin sizing and the watermark — and 200 years later their paper fed Gutenberg's press.
Source: content/entries/knowledge/paper.md