Part 2 · Earth and Fire
The Kiln
How to build a simple updraft kiln from clay, sand and straw, fire it to 900–1,100 °C, and judge the temperature by the colour of the glow. The kiln is the gateway to strong pottery, brick, lime, glass and metal.
- Difficulty
- ●●●●●
- Time
- One to two weeks to build and dry; 8–12 hours to fire; a day to cool
- Steps from zero
- 2 prerequisites →
The full path from nothing — 2 steps before this one
- Fire
- Finding and Preparing Clay
- The Kiln
Do them roughly in this order. See it on the tech tree →
Why it matters
An open fire loses most of its heat to the sky. A kiln is a fire in a box: it traps the heat, so the temperature keeps climbing, and it surrounds what you are firing so it heats evenly. Where a bonfire struggles to reach 800 °C for an hour, a simple clay kiln holds 900–1,100 °C for as long as you keep feeding it.
Those extra few hundred degrees change everything:
- Pottery comes out stronger, harder and less porous, and far fewer pots crack (see Pottery).
- Lime needs limestone held at about 900 °C for many hours — impossible in an open fire, routine in a kiln (see Lime).
- Fired bricks need 900–1,000 °C (see Bricks).
- Glazes and glass need 1,000–1,200 °C (see Glazes and Glass).
- Metal smelting uses the same ideas — an enclosed fire, a strong draught, insulating walls — pushed harder with Charcoal and Bellows (see Copper Smelting and Iron (the Bloomery)).
Learning to build a kiln, fire it, and read its temperature by eye is one of the most important skills in this book.
How it works
Hot gas rises. Hot air is lighter than cold air, so the column of hot gas inside a kiln floats upwards and out of the top, like a cork rising in water. As it leaves, it pulls fresh air in at the bottom, through the fire. This pull is called draught. The taller the hot column (a chimney adds height), the stronger the draught, and the hotter the fire burns.
An updraft kiln uses this directly. It has three parts stacked on top of each other:
- The firebox, at the bottom, where the wood burns. It has a stoke hole at the front, where you feed wood and air enters.
- The chamber, above, where the pots sit. A perforated floor (a clay floor full of holes) separates it from the fire, so flames pass through but pots do not sit in the embers.
- The flue, a hole in the roof, sometimes with a short chimney, where the gases leave.
The temperature you reach depends on four things:
- Insulation. Thick walls of clay mixed with straw hold heat in. Earth piled against the outside holds it in better still.
- Air. Too little air and the fire smoulders and smokes. Too much air — from a wide-open stoke hole or cracks — cools the kiln down. The art of firing is giving the fire just as much air as it can burn.
- Fuel. Dry, split wood burns fast and hot. Wet wood wastes its heat boiling off its own water. Thin, split softwood gives long, fast flames that carry heat up into the chamber.
- Time. A kiln is a big lump of clay that must itself be heated. It takes hours to climb.
What you need
For a small kiln with a chamber about 70 cm wide and 80 cm high — big enough for 15–30 medium pots per firing.
| Item | Amount | Notes |
|---|---|---|
| Kiln mix: clay | About 300 litres (15 bucketfuls) | Any sticky clay; does not need cleaning (see Finding and Preparing Clay) |
| Kiln mix: sand or grog | 300–600 litres | One to two times the volume of clay |
| Chopped straw, dry grass or dung | Several armfuls | Cut to 5–10 cm; makes the mix crack-resistant and insulating |
| Stones or fired bricks | Optional | For the firebox and to save clay |
| Broken pottery (sherds) | A heap | For the temporary roof |
| Sticks for formers | A few | To shape the arch over the stoke hole and the floor holes |
| Firewood | About 1 cubic metre stacked | Dry, split to wrist-thickness; softwood is best for the hot end of the firing |
The kiln mix is 1 part clay to 1–2 parts sand or grog by volume, with as much chopped straw as it will hold while still sticking together. Tread it with bare feet until even. Test a fist-sized ball: it should hold together when dropped from waist height onto hard ground, flattening but not falling apart.
Tip Use a slope. Dig the firebox into the side of a gentle bank, with the stoke hole on the downhill side. The earth around the firebox insulates it for free and saves half the building work. Choose a site that stays dry — a kiln on wet ground spends its heat boiling the soil.
Building the kiln
- Mark out a circle 110 cm across (the outside of the kiln). Clear the ground and stamp it flat.
- Dig the firebox. In the centre, dig a trench 40 cm wide and 40 cm deep, running from the back of the circle straight out past the front edge for another 60 cm. The part outside the circle is the stoke tunnel. Its outer end is the stoke hole — about 30 cm wide and 30 cm high. Line the trench walls with stones and kiln mix, or plaster them with 5 cm of kiln mix.
- Build the floor supports. Down the middle of the firebox, under the chamber, build a low wall of stones or kiln mix — a tongue — or a row of two or three pillars, to support the floor's middle.
- Lay the perforated floor. Bridge the firebox with a slab of kiln mix 8–10 cm thick, resting on the trench edges and the tongue. Before it sets, push sticks through it to make holes 3–4 cm across, about 10 cm apart all over — 30 to 40 holes. Pull the sticks out once the clay is stiff. About a fifth of the floor should be holes. (If you have fired bricks or clay bars, you can lay them across the firebox with finger-wide gaps instead.)
- Build the walls. Starting on the floor's edge, build a ring wall 15–20 cm thick with handfuls of kiln mix, pressing each handful down hard into the one below. Build no more than 20–30 cm per day; let each course stiffen before adding the next, or the wall slumps. Bring the wall to about 80 cm above the floor, curving slightly inward at the top.
- Add spy holes. In the wall, at two or three heights, leave holes about 3 cm wide, plugged with a clay stopper or a rolled-up piece of fired clay. Through these you will watch the colour of the fire.
- Arch the stoke hole. Above the stoke tunnel's outer end, shape an arch of kiln mix over a curved bundle of sticks, which will burn out in the first firing.
- Insulate. Pile earth around the outside of the walls, as high as you can, and pack it down. Every centimetre helps.
- The roof. For a small kiln, the simplest roof is rebuilt each firing: lay large broken pots and sherds over the loaded pots in a dome, then plaster over them with 5–8 cm of kiln mix and straw, leaving a flue hole 15–20 cm across in the centre. A chimney — a clay pipe or a tube of kiln mix 50–150 cm tall over the flue — improves the draught a great deal. Larger kilns can have a permanent dome with a side door that you brick up each time.
- Dry it. Let the kiln air-dry for at least a week under a rough roof of branches and leaves. Then light a small fire in the firebox and keep it going gently for one or two days. Steam will pour out. Cracks will appear — this is normal. Fill large cracks with kiln mix. The kiln is ready when a cold stone or pot held over the flue no longer fogs with moisture.
Loading the kiln
- Load only bone-dry ware (see Pottery).
- Put large, heavy pieces at the bottom and small ones on top. Stand the bottom layer on small stones or clay lumps so flame can pass beneath.
- Pots can touch and be stacked: bowls can rest rim-to-rim, small pots inside larger ones. Unglazed pots do not stick together.
- Leave paths for the flame. Do not block the floor holes or pack the pots so tight that gas cannot flow up between them.
- Put a few draw trials where you can reach them through a spy hole: small rings of the same clay, 3 cm across, that you can hook out with a long stick during firing to see how far the firing has gone.
- Build the roof of sherds and plaster over the top, as above.
Firing schedule
A typical firing to about 950 °C takes 8–12 hours in a small kiln, plus a day to cool. The rule: slow at the start, steady in the middle, hard at the end, slow to cool.
- Water smoking (0–200 °C), 2–3 hours. Light a small fire at the mouth of the stoke tunnel, not inside. Gradually push it inward. Clouds of steam come out of the flue. Hold a cold stone, a piece of metal or a fired sherd over the flue: if it fogs with moisture, water is still coming out. Do not hurry. Thick or large pieces need more time.
- Low heat (200–600 °C), 2–3 hours. When the cold-stone test stays dry, feed the fire fully inside the firebox and raise the heat steadily. Smoke may thicken as straw and other matter in the clay burn out. In the dark, the first faint red glow appears in the spy hole at around 500–550 °C. Do not rush past 573 °C: quartz grains in the clay change size suddenly here, and pots heated unevenly crack.
- Climbing (600–950 °C), 3–4 hours. Now feed the fire hard and often. Use thin, split, very dry wood. Add a few pieces at a time whenever the roar dies down and the flames at the flue shrink. Flames will lick out of the flue at the top. Watch the colour in the spy holes (below).
- Soaking (holding at the top), 30–60 minutes. When the spy holes show the colour you want, keep feeding just enough to hold it there. This lets the heat soak into the middle of thick pieces and into the cooler corners. You know heat is even when the pots and walls glow the same colour and the pots seem to disappear against the walls, with no shadows.
- Closing up. Stop feeding. Close the stoke hole with a stone slab or bricks and seal the gaps with mud. Cover the flue with a sherd. Shutting the kiln stops cold air rushing through and cracking the hot pots.
- Cooling: at least 12–24 hours. Do not open the kiln early. When you can rest your hand on the outside wall, open the flue; when you can touch the top of the roof, open the kiln. Pots taken out while hot can crack from cold air.
Note Reading the fire as you stoke. A steady, roaring sound and clear, flickering flames at the flue mean a good burn. Thick black smoke pouring from the flue after each stoking means too much wood at once and too little air — the kiln is starved and the temperature drops; stoke less, more often. If the temperature will not rise, check for big cracks letting in cold air, try drier or thinner wood, or add a taller chimney.
Judging temperature by colour
Without instruments, the colour of the glow is your thermometer. Everything hot enough glows, and the colour depends on the temperature, not on what is glowing: pots, walls and embers at the same temperature glow the same colour.
| Colour seen inside the kiln | Temperature (approx.) | What it means |
|---|---|---|
| No glow; only visible in total darkness as a faint grey-red | 450–550 °C | Clay is just turning to ceramic |
| Dark, dull red | 550–650 °C | Bonfire level; weak earthenware |
| Dull cherry red | 650–750 °C | Good low-fired pottery |
| Cherry red | 750–850 °C | Strong earthenware |
| Bright cherry to red-orange | 850–950 °C | Lime begins to burn; bricks firing |
| Orange | 950–1,050 °C | Good earthenware, bricks, lime |
| Yellow-orange | 1,050–1,150 °C | Glass melts; copper melts (1,085 °C) |
| Yellow | 1,150–1,250 °C | Stoneware begins; hard for a wood kiln |
| Pale yellow to white | 1,250 °C and above | Needs a very good kiln or bellows |
How to look:
- Judge in the same light every time — ideally at dusk or at night. In bright sunshine a kiln at 800 °C looks barely red; at night the same kiln looks bright cherry. Shade the spy hole with your hand.
- Look at the pots and the walls, not the flames. Flames are gas burning; their colour does not show the kiln's temperature.
- Pull out a draw trial with a long stick and drop it in water. If it is hard and rings, and does not soften when soaked, the firing has reached ceramic. Compare it with trials from earlier firings.
Melting markers. You can also place small "test lumps" in a broken sherd where you can see them through a spy hole:
- Common salt melts into a clear liquid at about 800 °C.
- Copper (a scrap or bead, see Copper Smelting) melts at 1,085 °C.
Later, small standard cones of clay that bend at known temperatures do the same job more exactly (see Pyrometric Cones and Kiln Temperature). If you have none of these, the colour chart and draw trials are enough. Traditional potters fired by eye for thousands of years.
How to tell it worked
- Pots ring clearly when tapped and do not soften in water.
- Fired pieces are evenly coloured, without dark grey cores when broken.
- Earthenware fired to orange heat (950–1,000 °C) is noticeably harder than bonfire pottery: a steel blade only just scratches it, and it soaks up much less water.
- Most of the load survives. In a well-run kiln, losses should drop below one pot in ten.
Note Troubleshooting. Pots at the top underfired, bottom ones fine → normal in an updraft kiln; put less important pieces at the top, soak longer, or add a chimney. Pots burst early in the firing → not dry, or water-smoking was too short. Cracks across pots that look sharp-edged and clean → cooled too fast; seal the kiln and wait longer. Temperature stalls below cherry red → wet fuel, too much air through cracks, firebox choked with ash (rake it out), or flue too small. Kiln walls crack badly → normal at first; patch with kiln mix after every firing. More straw and grog in the mix helps.
Dangers
Danger Burns and fire. A kiln's walls, ground and surrounding earth stay hot enough to burn for a full day after firing. Flames shoot from the flue and sparks fly. Build at least 5 metres from any roof, thatch, tree or stack of fuel, and never fire under a shelter.
- Bursting pots or wet kiln walls can blow apart. Stand clear of the stoke hole when the fire is first pushed in.
- Radiant heat. At orange heat, the stoke hole can burn exposed skin from a metre away in seconds. Wear leather or wet wool over arms and face when stoking. Feed wood with a quick movement and step back.
- Eyes. Staring into a white-hot kiln for long periods, firing after firing, damages the eyes over years. Look briefly; do not stare.
- Smoke and carbon monoxide. Never fire a kiln inside a closed building. Do not sleep close beside a cooling kiln in a hollow or pit where gas collects.
- Collapse. Old, cracked kilns can fall in. Do not climb on a kiln.
Going further
- Higher temperatures. A taller chimney, thicker insulation, drier and thinner wood, or air blown into the firebox with Bellows all push a kiln higher. Firing with Charcoal and bellows reaches well over 1,200 °C.
- Better walls. Walls of fired brick lined with heat-resisting clay last for hundreds of firings (see Bricks and Firebrick and Refractories).
- Better kiln designs. In a cross-draught kiln the fire is at one end and the flue at the other; in a downdraught kiln the flames rise, turn at the roof and are pulled down through the pots to a flue in the floor. Both heat more evenly and reach higher temperatures. Long kilns built up a hillside (Chinese "dragon kilns", Japanese and Korean climbing kilns) reached 1,250 °C and above, hot enough for Stoneware and Porcelain.
- Uses. The same kiln burns Lime, fires Bricks, and, with a crucible, melts Glass and Glazes.
How it was first done
For thousands of years after pottery was invented, all of it was fired in bonfires and pits. The first enclosed updraft kilns, with a firebox below a perforated floor, appear in Mesopotamia and the neighbouring Near East by around 6000 BC. Within a few thousand years the same kind of kiln, with more draught, was being used to smelt copper. Chinese potters built ever longer and hotter kilns, reaching temperatures above 1,200 °C over two thousand years ago — the start of stoneware and, later, porcelain. Until the 20th century, nearly every kiln in the world was fired by someone who judged the temperature by the colour of the glow.
Source: content/entries/earth/kiln.md