◆ Rebuild

Part 5 · Cloth and Clothing

Felt

Wool that has been wetted, soaped and rubbed until its fibres lock into a dense, warm, windproof sheet — no spinning, no loom. Felt makes hats, boots, rugs, tent walls and insulation, and it was probably the first fabric people ever made from animal fibre.

Difficulty
●●●●●
Time
A small mat in 2–3 hours; a pair of boots in a day; a tent-sized sheet in a day with a team
Steps from zero
4 prerequisites →

You need first

Wool

This unlocks

Insulation and Keeping Buildings Warm or CoolHats, Gloves, Scarves and Stockings

Raw materials

wool
The full path from nothing — 4 steps before this one
  1. Stone Tools
  2. Farming from Seed
  3. Keeping Animals
  4. Wool
  5. Felt

Do them roughly in this order. See it on the tech tree →

Why it matters

Spinning and weaving (Spinning and Weaving Cloth) turn wool into cloth, but they take weeks of skilled work for every garment. Felt turns raw wool into a thick, strong sheet in an afternoon, with nothing but hot water, soap and your hands. It needs no tools at all.

Felt is one of the warmest materials you can make. It traps air, it blocks wind, it sheds rain, and — because it is wool — it stays warm when damp. It does not fray, so it can be cut to any shape and used without hemming. With felt you can make:

The same process, applied to woven wool cloth, is called fulling: it shrinks and thickens the cloth so it becomes dense and weatherproof (see Spinning and Weaving Cloth). If you understand felting you understand both.

How it works

Look at a wool fibre under a lens (Lenses, The Microscope) and you will see that its surface is covered in tiny overlapping scales, like the tiles on a roof or the scales on a fish, all pointing towards the tip of the fibre.

A WOOL FIBRE, GREATLY MAGNIFIED Scalesoverlap like roof tiles,edges toward the tip Root end Tip slides easily root-first scales catch: will not slide Carded woolloose, fibres side by side Feltfibres crept and locked together
Fig. 1 Why wool felts. Its scales let a fibre slide easily towards its root end but catch when pulled the other way. Shaken and rubbed, every fibre creeps root-first and the fibres tangle into a mat that cannot come apart.

Rub a fibre between finger and thumb and it will creep in one direction only — root first — because the scales let it slip one way and catch the other way, like a ratchet. In a heap of wool, every fibre is crawling, each in its own direction, under every push and squeeze. They wind round each other, hook their scales together, and pull the whole mass tighter and tighter. The result is felt: a tangle so dense that it cannot be pulled apart.

Three things make it happen faster:

  • Heat (warm to hot water, 40–60 °C) softens the fibres and makes them slide.
  • Alkali — soap (Soap) — makes the fibres swell and their scales lift, and lubricates them so they move.
  • Agitation and pressure — rubbing, rolling, throwing, treading — drive the movement. The more you work, the more it shrinks and the firmer it gets.

Felting cannot be undone. That is why a wool sweater washed hot shrinks to child size. It is also why felt is so strong.

Which fibres felt. Sheep's wool felts best, especially fine, crimpy wool (from breeds like Merino, Shetland and most "down" and mountain breeds; a fibre you can barely see). Coarse, straight, hairy wool felts slowly. Kemp — the stiff, chalky-white, brittle hairs in some fleeces — never felts. Camel, yak and alpaca fibres felt partly and are best mixed with sheep's wool. The fine under-fur of rabbits, hares and beaver makes the finest hat felt. Plant fibres (linen, cotton, hemp) do not felt at all — they have no scales.

What you need

Item For a 50 × 70 cm mat Notes
Wool, washed and carded 250–350 g Fluffy and open, not in lumps. See Wool
Hot water 5–10 litres 40–60 °C: hot, but you can hold your hand in it
Soap A handful of soft soap, or a thumb-sized lump of hard soap grated into the water Any plain soap. See Soap
Reed or grass mat Bigger than the layout A mat of reeds, thin sticks or straw lashed side by side (Baskets and Containers); or an old blanket
Thin cloth As big as the layout Old linen or a loose weave, to lay on top while rubbing
Pole 4–5 cm thick, longer than the mat is wide For rolling
Sprinkler A gourd or pot with holes poked in it, or a bundle of twigs dipped and shaken
Vinegar (optional) A cup For the final rinse (Fermentation)

How much wool? Wet-felted wool shrinks by roughly 20–40% in length and width. Lay out an area about a third bigger in each direction than the finished piece. For weight, allow roughly 0.6–1 kg of clean wool per square metre of finished felt 3–4 mm thick. A 1-cm felt for a tent wall or boot needs 2–3 kg per square metre.

Where to find it

  • Wool comes from sheep, shorn once a year in late spring (Wool, Keeping Animals). Felt does not need the best fleece: belly wool, short second cuts and the shorter bits left after combing all felt well. Wash out the grease (lanolin) first — greasy wool barely felts.
  • Other animal fibre: goat down, camel, yak, dog undercoat, and the fur of rabbits and hares. Pluck or comb it; mix it about half and half with sheep's wool.
  • Soap: make it from wood ash lye and fat (Lye and Potash, Soap). In a pinch, a strong lye made from wood ash and water works, but it is harsh on hands and on the wool — dilute it until it barely feels slippery between your fingers.

Method 1: A flat sheet of felt by hand

1. Lay outthin wisps, overlappinglike tiles; each layer atright angles to the last 4 thin layers ≈3–4 mm of felt 2. Wet and rubhot soapy water, 40–60 °C;rub through a cloth, gentlyat first, 5–10 min a side until the pinch test showsthe wool lifts as a skin 3. Rollround a pole inside a mat;100 rolls, then turn ¼ andrepeat, both sides press with forearms 4. Fullthrow it down hard, kneadit, dip it hot, until it hasshrunk 20–40%, and firm then rinse and dry flat
Fig. 2 Making flat felt. Lay thin wisps of wool in crossing layers; wet with hot soapy water and rub gently until the surface holds together; roll it up in a mat and roll hundreds of times from every direction; then throw and knead it until it is firm.
  1. Lay out the mat on a table, a board or clean ground. Mark the layout size (finished size plus a third) with sticks or a line of thread.
  2. First layer. Pull thin wisps from the carded wool — about as long as your hand, so thin you can see through them. Lay them in a row, all pointing the same way, each overlapping the one before by half, like roof tiles. Cover the whole area.
  3. Second layer at right angles to the first. Then a third layer the same way as the first, and a fourth across. Four thin layers make about 3–4 mm of felt; for thicker felt, add more pairs of layers. Thin, even layers matter more than anything else. Hold your hand flat just above the wool: it should be an even, cloud-like heap 4–8 cm deep, with no gaps or thick lumps.
  4. Decorate (optional). Lay wisps of dyed wool (Dyes and Mordants) on top in a pattern; they will felt into the surface.
  5. Wet it. Lay the thin cloth on top. Sprinkle the hot soapy water evenly all over, starting in the middle. Press down with flat hands to push out the air. Add water until all the wool is wet through and dark, but not floating in a puddle.
  6. Rub gently. With flat, soapy palms, rub the cloth in small circles, starting with almost no pressure and slowly pressing harder. Work every part, especially the edges (fold the loose edges in neatly first). Rub for 5–10 minutes each side; turn the whole thing over and rub the other side.
  7. The pinch test. Pinch a few surface fibres and lift. If single fibres pull away, keep rubbing. When the surface lifts as a whole skin, the wool has become prefelt — it hangs together, but is still soft and loose.
  8. Roll. Remove the cloth. Lay the pole on one end of the mat and roll the mat up tightly around it with the felt inside. Tie the roll with cord in two places. Roll it back and forth on the table under your forearms, pressing hard — 100 times. Unroll, turn the felt a quarter-turn, smooth out any wrinkles, roll up again and roll another 100. Do all four directions, then turn the felt over and do all four again. Add hot soapy water whenever it cools.
  9. Full it. Now treat it roughly. Bunch it up, dip it in hot water, and throw it down hard on the table, 20 times, then open it and pull it straight. Knead it like bread dough. It will shrink visibly. Measure often and stop when it is the size you want. Pull it gently into shape between throws. If it shrinks too much in one direction, work it more in the other.
  10. Rinse. Rinse out the soap in warm water, then cold. A cup of vinegar in the last bucket neutralises the alkali and leaves the wool softer.
  11. Shape and dry. Squeeze (don't wring) out the water, pull straight, and dry flat in the shade. Felt dries in a day or two in good weather.

Method 2: Big felts for tents and rugs

Big felt — for a ger wall, a floor rug, or a sleeping mat — is made the same way but by a team, the way it has been done on the steppes of Central Asia for thousands of years.

  1. Open the wool. Spread the washed fleece on a hide or clean cloth and beat it with a pair of flexible sticks (willow rods) for an hour to fluff it and shake out dirt. This replaces carding.
  2. Lay it out on a large reed mat, a hide, or an old felt (the "mother felt", which acts as a mould). Spread it evenly 10–20 cm deep. Several people work at once, each on a section, checking for thin spots.
  3. Wet it with hot water (soap is optional when the wool is fine and the work is long), sprinkled from a ladle or a bundle of twigs.
  4. Roll it tightly round a long pole, wrap the roll in a wet hide or another felt, and tie it firmly.
  5. Drive it. The roll is then rolled to and fro for hours: by a line of people pushing it with their feet, or by tying a rope to each end of the pole and dragging it across the grass behind a horse or camel. Unroll it every hour or so, check it, wet it again, and roll from the other end.
  6. Finish by hand. The felters kneel in a row and press and roll the felt with their forearms, working along it, until it is firm. Then it is dried in the sun.

Two or three layers of 1–2 cm felt, tied over a frame of wooden lattice walls and roof poles, make a ger that stays warm at −30 °C with a small stove inside.

Method 3: Seamless felt — boots, hats, bags and mittens

Felt can be made into hollow shapes with no seams, by laying wool around a flat resist — a waterproof template that stops the two sides felting to each other.

1. Lay the wool on the resist wool hangs2–3 cm overevery edge Resistrawhide, oiled leather or bark,25–40% bigger than the boot 2. Fold round, lay the other side second series of layers first series resist Each series wraps round the edge, sono seam forms. 3 or more layers a side. 3. Cut, remove, shape last cut the top open, pull outthe resist, full the bootonto a wooden last
Fig. 3 Seamless felting around a resist. Wool is laid on one side with an overhang, folded round the edge, and laid on the other side, several times. Once it has felted, the opening is cut, the resist is taken out, and the shape is fulled on a form.
  1. Make the resist. Cut the shape you want — a boot in side view, a mitten, a bag, a hat outline — 25–40% bigger in every direction than the finished size. Use a thin, flexible, waterproof sheet: rawhide or thin oiled leather (Hides and Leather), oilcloth, or a sheet of birch bark. For boots, the resist is the outline of the boot (foot and leg) seen from the side, with extra room at the toe.
  2. Lay the first side. Put the resist on the mat. Lay two thin layers of wool on it at right angles, letting the wool hang 2–3 cm over every edge.
  3. Wet and flip. Wet with hot soapy water, press it flat, then carefully turn the whole thing over (cover with a cloth to turn it). Fold the overhanging wool neatly around onto the second side.
  4. Lay the second side the same way, with overhang, wet it, flip it back and fold the overhang over the edges. Repeat until you have 3 layers each way on each side — more for boots. Boots need felt 6–10 mm thick when finished; use about 1 kg of wool for a pair of adult knee boots.
  5. Rub both sides and the edges, as for flat felt, until the pinch test shows prefelt. The edges are where seamless felt fails; rub them hard, pressing the fold.
  6. Cut the opening (the top of the boot, the wrist of a mitten) with a knife, and pull out the resist.
  7. Full it from the inside. Put your hand inside and rub the inside surfaces. Throw it, knead it and roll it. It will shrink round the shape.
  8. Shape on a form. Pull the wet felt over a form and keep working it until it fits tightly: a carved wooden last for boots (Footwear), a round block of wood, a smooth stone or an upturned clay pot for a hat (Pottery). Leave it on the form to dry.

Tip Fulled knitting. A hat, mittens or slippers knitted about a third too big in wool (Knitting, Crochet and Netting) and then washed hot and rubbed will shrink into a dense, windproof felt. It is quicker to make than laid-out felt for small things, and very hard-wearing.

How to tell it worked

  • The pull test. Grip the felt with two hands 5 cm apart and pull. Good felt stretches a little but does not thin out or tear. If fibres slide apart, it needs more fulling.
  • The light test. Hold it up to the sky. It should look evenly dense — no thin, bright patches.
  • Surface. Rub it with your palm. It should feel firm and smooth, not loose and fluffy.
  • Water. Drip water on it. Good, firm felt sheds most of it at first, and the water soaks in only slowly.
  • Size. It should have shrunk by roughly a fifth to a third from the layout.

Note Troubleshooting. Nothing happens after 20 minutes of rubbing → water too cold, wool still greasy, or the wool is coarse or kempy. Use hotter water, more soap, wash the wool again, or mix in finer wool. Slippery, foaming and still not felting → too much soap; the fibres just slide. Rinse some out. Holes and thin patches → uneven layout. Lay a wisp of dry wool over the hole, wet it and rub it in while the felt is still at the prefelt stage. Hard creases → the felt was rolled up with wrinkles in it. Smooth it every time you unroll; creases set permanently once fulled. Seamless piece split at the edge → the overhang was too short or the edges were not rubbed. Patch with dry wool and keep the edges well worked. Shrunk too much in one direction → it was rolled more one way. Roll the other way; wet felt can also be stretched a little while still hot.

Dangers

Danger Anthrax from raw wool. Wool, hair and hides from animals that died of disease can carry anthrax spores, which survive in fleece and soil for decades. Breathing the dust when sorting or beating wool causes "woolsorters' disease", which is usually fatal; spores in a cut cause a black, painless sore with swelling. Never use wool or hair from an animal found dead or that died of sickness. Beat and sort dry fleece outdoors, upwind, and wash your hands and face afterwards. See Infectious Diseases and Animal Health.

  • Scalds. Water hotter than about 60 °C will burn your hands in seconds. Test with your elbow first, as for a baby's bath.
  • Cracked, burned skin. Strong soap and lye attack skin. Use mild soap, rinse your hands often, and grease them afterwards with fat or wool grease.
  • Mercury. From the 1600s to the 1940s hat-makers treated fur with a mercury solution so it would felt faster. It poisoned them — trembling, loss of memory and personality changes, the "mad hatter". Never use mercury for felting. Soap and work do the job.
  • Back and shoulder strain from long rolling. Work at a table at hip height, take turns, and use the big tools (feet, animals) for big felts.
  • Moths and mould destroy stored felt. Dry it completely before storing; keep it with cedar, juniper or wormwood, and air it in the sun.

Going further

  • Fulling cloth woven from wool is the same process: soak, soap, pound. Fulling mills driven by water power (The Waterwheel, The Watermill) with heavy wooden hammers were among the first factories in Europe.
  • Hat felt from rabbit or beaver fur, shaped over a wooden block with steam, makes the felt hats that kept rain off people for 400 years (Hats, Gloves, Scarves and Stockings).
  • Pressed and needle felts: industrial felt is made by machines that pound or punch the fibres with barbed needles, and it is used for gaskets, wicks, polishing, and the felts of paper machines (Paper) and piano hammers.
  • Patterned rugs (the Kyrgyz shyrdak) are made by cutting two felts of different colours in the same pattern and sewing the pieces of one into the gaps of the other (Sewing, Needles and Thread).

How it was first done

Felt is so simple that it was probably discovered many times — wool socks and bedding packed into shoes would have felted by themselves with sweat and walking. Because felt rots away, early evidence is scarce. The most famous early felts come from the frozen tombs of Pazyryk in the Altai Mountains of Siberia, from about the 4th and 3rd centuries BC: saddle cloths, wall hangings with appliquéd riders, stockings and stuffed felt swans, all perfectly preserved in ice. Greek and Chinese writers describe the felt tents and clothing of the steppe peoples, and the Mongols of the 13th century carried their felt gers across half of Asia. In Europe, felt hats became a major industry from the 1500s; the poisoning of hatters by mercury was finally banned in the United States only in 1941.

Source: content/entries/textiles/felt.md