◆ Rebuild

Part 13 · Electricity

Insulators, Cables and Electrical Fittings

The small parts that hold, join and end every electric circuit — porcelain and glass insulators for lines, cleats, wall tubes and bushings, cables and how to joint and terminate them, ceiling roses and lamp holders, junction boxes and extension leads — how to make each, and how to do it so that nothing overheats.

Difficulty
●●●●●
Time
A day to pattern and mould a set of fittings; a week to dry and fire them; an hour to joint and terminate a cable properly; ten minutes to fit a ceiling rose
Steps from zero
29 prerequisites →

You need first

Wiring and Electrical SafetyStoneware and Porcelain

This unlocks

—
The full path from nothing — 29 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Lime
  13. Bricks
  14. Lye and Potash
  15. The Wheel and Axle
  16. Glass
  17. Firebrick and Refractories
  18. Bellows
  19. Gears
  20. Glazes
  21. Copper Smelting
  22. Iron (the Bloomery)
  23. The Waterwheel
  24. Stoneware and Porcelain
  25. Blacksmithing
  26. Magnets
  27. Copper Wire
  28. The Generator
  29. Wiring and Electrical Safety
  30. Insulators, Cables and Electrical Fittings

Do them roughly in this order. See it on the tech tree →

Why it matters

Every circuit needs parts that hold the wire off walls and poles, carry it through walls and cases, join it, end it at a lamp or appliance, and let a lamp hang or a tool plug in. These fittings are where the trouble is: a wire in open air rarely fails, but joints, terminals and holders are where heat builds up, fires start and people touch live metal.

Wiring and Electrical Safety covers wire sizes, fuses, earthing and switches. This chapter makes the parts in between, from porcelain (Stoneware and Porcelain), brass (Zinc and Brass), copper (Copper Wire) and rubber (Rubber), for houses, workshops, the The Telegraph, The Telephone, Power Lines and Distribution and Electric Fences.

How it works

Three rules make a fitting safe.

1. Keep live parts apart, along the surface as well as through the air. Electricity leaks across the surface of an insulator more easily than through it, especially when the surface is damp or dirty. The distance along the surface between two metal parts at different voltage is the creepage distance. Make it long:

Where Minimum surface path between live parts, or live and earth
Indoors, dry, 110–250 V 6 mm on glazed porcelain; 10 mm on slate, marble or dry hardwood
Indoors, damp (barns, wash-houses) 15–20 mm, glazed porcelain or glass only
Outdoors, on lines About 20–25 mm per 1,000 V, with sheds that keep part dry

Ridges, grooves and sheds (downward skirts) lengthen the path without making the fitting bigger, and the underside of a shed stays dry in rain.

2. Make every contact tight, clean and large. A joint or terminal has a small resistance where the metals touch. Heat at a contact = current² × resistance. A loose joint of only 0.05 Ω carrying 10 A makes 5 watts — as much as a small soldering iron — in a space the size of a pea, inside a box, for hours. That chars wood, softens rubber and loosens the joint further, which raises the resistance: a joint that has started to overheat gets worse until it burns. Clean metal, firm pressure, a large contact area, and solder where the joint cannot be screwed, stop this.

3. Keep heat away from insulation. Each insulating material has a highest safe temperature:

Material Safe up to about Use
Gutta-percha 40 °C (softens) Underwater and underground cable only
Natural rubber, vulcanised 60 °C Cables, flex
Varnished cotton, wax 80–90 °C Wire covering, tape
Hardwood, fibre 100 °C (chars above) Low-voltage bases, boxes
Ebonite, early plastics 70–100 °C Lamp holder bodies, plug tops (Early Plastics)
Slate, marble 300 °C+ Switch and fuse bases
Porcelain, glass, mica 500 °C+ Insulators, lamp holders, heater parts

What you need

Item For Notes
Electrical porcelain body Insulators, cleats, tubes, roses, holders About 45 kaolin and ball clay, 30 feldspar, 25 quartz, by weight (Stoneware and Porcelain)
Plaster of Paris Moulds Gypsum and Plaster of Paris
Steel dies and a screw or lever press Dust-pressed small parts Presses, Punches and Dies
High-temperature kiln, glazes 1,250–1,350 °C The Kiln, Glazes
Brass strip, rod and screws Terminals, holders, contacts Zinc and Brass, Screws, Nuts and Bolts
Phosphor bronze or spring brass Plungers, contact springs Springs
Copper wire, tinned Conductors, binding wire Copper Wire, Tin and Pewter
Rubber, cotton tape, varnish Insulation Rubber
Solder and rosin Joints Soldering and Brazing
Bitumen or pitch Filling outdoor and buried joint boxes Tar, Pitch and Glue
Glass press and moulds Glass insulators Bottles, Drinking Glasses and Glassware

Where to find it

Kaolin (white china clay from rotted granite), feldspar (pink or white blocky crystals in granite) and quartz make porcelain (Finding and Preparing Clay, Rocks and Minerals). Slate splits into flat sheets; marble saws and drills easily; mica splits into clear flexible sheets from pegmatite veins. Rubber and gutta-percha are tree latexes (Rubber); bitumen seeps from the ground near oil fields or is made from tar (Tar, Pitch and Glue).

Making porcelain fittings

Every porcelain fitting is made one of three ways.

  • Thrown or turned. Large round insulators are thrown on the wheel (The Potter's Wheel) and then turned leather-hard on a lathe-like jigger with a profile tool to an exact shape. Threads for a pin can be formed with a threaded wooden former.
  • Slip-cast or pressed in plaster. Pour liquid clay (slip) into a plaster mould; the plaster soaks up water and a skin forms. Pour out the rest (hollow parts) or let it fill (solid parts). Or press soft clay into two halves of a plaster mould by hand.
  • Dust-pressed. For small exact parts — cleats, ceiling rose bases, lamp holder interiors, terminal blocks — grind dry porcelain body, damp it with 6–8 % water so it just holds together when squeezed, fill a steel die, and press it hard with a screw or lever press. The part comes out ready to dry and fire, with holes and slots sharp and to size.

Allow for shrinkage. Porcelain shrinks about 12–15 % in drying and firing. Make every mould and die that much bigger, and every hole that much bigger than the screw that must pass through it. Test-fire a sample bar marked 100 mm and measure it.

Fire to 1,250–1,350 °C until the body is glassy right through (Stoneware and Porcelain); glaze everything that will be outdoors or damp. Break one piece from each firing: the broken face should be smooth and glassy, and a drop of ink on it should not soak in. Porous porcelain soaks up water and conducts.

Insulators for lines

Pin insulator wire in the top groove Shedsundersides stay dry Leakage pathlong, along the surface threaded pin crossarm Spool on a bolt and bracket,for line ends and corners 50–75 mm across Egg (strain) loops at right angles;porcelain squeezed,not pulled guy Porcelain cleatfrom the front 40–60 mm one screw clampsboth halves Wall tubeinside outside tube slopes downto the outside drip loop
Fig. 1 Left: a pin insulator cut through, screwed on a pin. The dashed line is the leakage path from wire to pin: up over the top, down the outside, round under each shed and up again — far longer than the insulator is tall. Middle: a spool (shackle) insulator on a bolt, for ends and corners. Right: an egg (strain) insulator in a guy wire; the two loops pass through it at right angles, so the porcelain is squeezed, not pulled, and if it breaks the loops still hold. Bottom: a two-wire porcelain cleat, and a wall tube sloping down to the outside with a drip loop.

How they are mounted and tied on the pole is in The Telegraph and Power Lines and Distribution. Here are the shapes and sizes.

The pin insulator

A dome with a groove round its top or side for the wire, a threaded hole in its base for a wooden or iron pin, and one or more downward sheds.

  • Low voltage (up to about 1,000 V): 80–100 mm tall, 70–90 mm across, one shed, wire groove 12–15 mm wide.
  • For 10,000–15,000 V: 150–200 mm tall and across, two or three sheds, walls 15–25 mm thick. Thick porcelain must be fired slowly and completely; any unfired core will crack in frost.
  • The pin thread: form it in the clay with a threaded former, or cement the insulator onto an iron pin with sulphur, lead or neat cement mortar. A wooden pin is screwed in with a tarred cloth wrapping.

Glass insulators

Pressed glass is clear, so you can see a crack, and smooth, so rain washes it clean. Press them in a two-part cast-iron mould with a threaded plunger that forms the pin thread inside (Bottles, Drinking Glasses and Glassware); unscrew the plunger while the glass is still soft enough not to crack but stiff enough to keep its shape. Anneal them very slowly — at least 24 hours — since they are thick. Use soda-lime glass of a good, durable batch: poor glass grows a white crust and leaks in time.

Spool and strain insulators

  • The spool (shackle) insulator: a glazed porcelain reel 50–75 mm across and 60–75 mm long, with a hole for a 12–16 mm bolt through a bracket. It takes the pull where a line ends, turns a corner or comes down to a house.
  • The egg (strain) insulator: an oval of porcelain 60–90 mm long with two holes at right angles. One end of the guy wire or aerial loops through one hole, the other through the other hole. The porcelain between the loops is squeezed, which porcelain withstands well, instead of stretched, which it does not. If it shatters, the loops still interlock and the guy does not fall onto the line.

Cleats, tubes and bushings

Porcelain cleats hold indoor wires a fixed distance apart and off the wall. A cleat is two flat pieces, about 60 × 25 × 12 mm each, with matching grooves across them for two or three wires at 40–60 mm spacing; one screw through the middle clamps the wires between the halves. Fix cleats every 1 m on walls and 75 cm on ceilings. A knob — a reel about 25 mm across with a screw through its centre — does the same for a single wire.

Wall tubes carry a wire through a wall, floor or beam. Make them 10–30 cm long, bore 8–12 mm for one wire, flared or with a collar at one end. One wire per tube. Through an outside wall, slope the tube down towards the outside and leave a drip loop in the wire outside, so water runs off the bottom of the loop instead of following the wire indoors.

Bushings carry a conductor through a metal case, a transformer tank, or anything earthed (The Transformer). A bushing is a porcelain tube with a shoulder that sits in the hole and a nut or a cemented collar to hold it; outdoors it has sheds. For low-voltage appliances, a rubber grommet or a fibre bushing round the cord where it enters a case stops the edge of the hole cutting the insulation (Electric Kettles, Irons, Heaters and Cookers). For heaters and lamps, use mica washers and porcelain beads where heat would char rubber.

Cables

A cable is one or more insulated conductors bound into one. Flexible cord (flex) is a cable of many fine wires for anything that moves.

  • Conductors. Solid wire for fixed runs; for flex, many fine strands — 0.75 mm² is 24 strands of 0.2 mm (Copper Wire).
  • Insulation. Two layers of vulcanised rubber, then cotton braid soaked in wax or varnish. Tin the copper first (Tin and Pewter): the sulphur in vulcanised rubber blackens bare copper and makes the rubber sticky.
  • Sheath. Pitch-soaked cotton braid round the cores; underground, a lead sheath, or rubber cable in an iron pipe; for heavy duty, iron wire armour over the lead.
  • Colours tell the cores apart: dye the cotton braid of each core, for example red for live, black for neutral and green for earth, the same scheme as the thread markings in Wiring and Electrical Safety. Use one scheme everywhere and write it in the logbook.
  • Gutta-percha is excellent under water and underground, where it stays cool and dark, but softens in the sun and cracks in air. Use it for submarine and buried cables only (The Telegraph).

Cable joints and terminations

Western Union splice solid house wire: cross, then 5+ tight turns each side then solder right through and tape Britannia joint line wire under tension: ends turned up, bound with 1 mm tinned wire, soldered overlap 75–100 mm Tee joint a branch: 6–8 close turns round the main wire branch main Terminations Eyebent clockwise,tightening closes it Strandedtwisted, undera washer Cable lugend sweated inwith solder
Fig. 2 Joints and ends. Top left: the Western Union splice for solid house wire, each end wound five or more turns round the other, then soldered. Top right: the Britannia joint for line wire, overlapped with turned-up ends and bound with fine tinned wire, then soldered. Bottom left: a tee joint. Bottom right: terminations — a wire eye bent clockwise round a screw so tightening pulls it in, a stranded end twisted and held under a washer, and a soldered cable lug.

Strip each end with a knife held almost flat, like sharpening a pencil, so you never nick the copper; a nick becomes a break. Scrape the copper bright.

Joint Where How
Western Union splice Solid house wire, end to end Cross the ends, wind each 5 or more tight turns round the other (Wiring and Electrical Safety)
Britannia joint Hard line wire under tension Overlap the ends 75–100 mm, turn up the last 5 mm of each, bind the overlap tightly with 1 mm tinned copper wire, then solder
Tee joint A branch off a run Wind the branch wire 6–8 turns round the main wire, turning it with pliers so the turns lie close
Married joint Stranded cable Splay and interleave the strands of both ends, then wind each set of strands round the other cable

Solder every joint with rosin flux, never acid flux or "killed spirits", which keeps eating the copper under the tape. Heat the joint, not the solder; the solder should run right into the turns (Soldering and Brazing).

Insulate with two layers of rubber tape (it fuses to itself), then two layers of varnished cotton tape, each overlapping by half, carried 25 mm past the bare copper. Outdoors or underground, put the joint in a cast-iron or glazed clay box and fill it with hot bitumen; heat it gently so the compound runs into every gap, and top it up as it cools and shrinks.

Terminations are where a wire meets a screw:

  • Solid wire: bend an eye with round-nosed pliers, clockwise, so tightening the screw closes the eye instead of pushing it out. Put a washer under the screw head.
  • Stranded wire: twist the strands tight, fold the end back on itself, and clamp under a washer or in a pillar terminal. Do not rely on solder alone under a screw: soft solder slowly flows under pressure, the clamp loosens, and the joint heats. If you tin the end, check the screw again after a week.
  • Large cables: sweat the end into a cable lug — a short copper tube closed at one end into a flat tongue with a bolt hole — filled with solder.
  • Cord grips: every portable cord must be clamped by its sheath where it enters a fitting, so a pull on the cord never pulls on the terminals.

Lamp holders and ceiling roses

Ceiling rosecut through, cover lowered Bayonet lamp holderexploded joist fixed wiring Porcelain base Terminals10 mm apart Anchor lugstake the weight screws on Cover Flex≤ 3 kg on 0.75 mm² Cap, cord gripclamps the flex covering Porcelain insert two spring plungers Brass sleeve22.5–23 mm inside L-slot (one each side) shade ring Lamp cap22 mm, two pins;contacts on the end
Fig. 3 Left: a pendant ceiling rose, opened. The porcelain base screws to a ceiling joist; the fixed wires come through its back to brass terminals; the flexible cord leaves through the cover, knotted or hooked over two anchor lugs so the lamp hangs from the porcelain, not the terminals. Right: a bayonet lamp holder, exploded — cord grip cap, porcelain insert with two spring-loaded plungers, brass sleeve with two L-shaped slots, and shade ring — above the bayonet cap of the lamp.

The lamp holder

It must hold the lamp, carry current to its cap, and stand the heat of the lamp just below it.

The bayonet holder is the easiest to make well. The lamp cap (The Light Bulb) is a brass sleeve 22 mm across with two short pins sticking out opposite each other and two soldered contacts on its end.

  1. Sleeve. Roll a brass tube 22.5–23 mm inside diameter, 30–35 mm long, from sheet 0.5–0.7 mm thick, and solder the seam (Sheet Metal and Rolling). Cut two L-shaped slots opposite each other in its open end, 3.5 mm wide: down 8 mm, then round 5 mm. The lamp's pins go down the slots, turn and lock.
  2. Insert. A porcelain or ebonite disc that fits inside the sleeve, with two holes for plungers: brass pins 3 mm across with a spring behind each (phosphor-bronze or brass spring wire). They push up against the lamp's contacts and press the pins up into the hooks of the slots, holding the lamp firm.
  3. Terminals. A brass screw terminal behind each plunger, with at least 6 mm of porcelain between them.
  4. Cap and cord grip. A threaded top cap that screws onto the sleeve, with a hole for the cord and a grip that clamps the cord's covering.
  5. Shade ring. A thread on the outside of the sleeve and a ring to hold a glass or metal shade.
  6. Earth. A metal holder must have its sleeve connected to earth, or be covered in an insulating skirt.

The screw holder (Edison type) takes a lamp cap with a coarse thread 27 mm across, pitch about 3.6 mm. The thread is a brass shell rolled to shape, and the second contact is a spring tongue in the centre of the base. Always connect live to the centre contact and neutral to the shell, so a finger touching the thread of a half-screwed lamp touches only neutral.

Good holder: the lamp goes in firmly and does not wobble; after an hour with a 100 W lamp, the cord grip and cap are warm but not hot to hold, and the porcelain shows no discolouring.

The ceiling rose

Where the fixed wiring meets the hanging flex for a pendant lamp.

  1. Base. A round porcelain or hardwood block 70–90 mm across and 25–30 mm deep, with two fixing holes to screw into a joist or a batten between joists — never into plaster alone.
  2. Terminals. Two or three brass terminals on a porcelain bridge inside: live, neutral and (for a loop-in rose) a spare to carry the live on to the next lamp. Keep 10 mm between them.
  3. Anchor. Two small lugs or a hole in the porcelain bridge that the flex is hooked or knotted round before it reaches the terminals.
  4. Cover. A porcelain or turned-wood cup that screws over the base, with a hole for the flex.

The flex carries the lamp's weight: at most 2 kg on 0.5 mm², 3 kg on 0.75 mm², 5 kg on 1 mm². A heavier fitting hangs from a chain or hook in the joist, with the flex looped loosely alongside.

Junction boxes

A junction box is a closed box where wires meet on screw terminals instead of being joined loose in the wall. Use one for every branch and every joint inside a building that is not soldered and taped.

  • Body: glazed porcelain or fired clay, slate, or iron (earthed) — never bare wood for anything above 25 V. Inside, at least 75 mm across and 35 mm deep, so the wires are not crammed.
  • Terminal block: a bar of porcelain with brass tunnel terminals, each tunnel taking the ends of two or three wires under one or two screws.
  • Entries: smooth holes or bushed entries, one per cable.
  • Lid: screwed on, never nailed, and always reachable: never plaster over a junction box.
  • Outdoors and in damp places: an iron box with a gasket, or a joint filled with bitumen as above.

Extension leads

A plug, a length of flex and a socket (Wiring and Electrical Safety), for reaching a tool or lamp away from a fixed outlet.

  1. Flex thick enough for the load: 0.75 mm² up to 5 A, 1.5 mm² for 10 A, 2.5 mm² for 15 A; check voltage drop on long leads (Wiring and Electrical Safety).
  2. Three cores, with the earth unbroken from plug pin to socket.
  3. A tough socket housing of rubber, hardwood or porcelain, contacts sunk out of reach of fingers; cord grips at both ends.
  4. Plug at the supply end, socket at the far end — never a plug at both ends, which leaves live pins bare.
  5. Do not use it coiled. Flex wound on a drum cannot shed heat: a fully wound reel should carry no more than a quarter to a third of its rated current.
  6. Check hard-used leads weekly for cuts, kinks, slack grips and warm plugs.

How to tell it worked

  • Hand test under load. Run each circuit at its full load for an hour. Then switch off and touch each joint box, terminal, rose, holder and plug with the back of your fingers. Warm is acceptable; too hot to hold for five seconds is a fault. Find and remake it.
  • Insulation test. With everything disconnected, put 100 V or more from a battery through a sensitive meter between each conductor and earth, and between conductors (Measuring Electricity, Electric Kettles, Irons, Heaters and Cookers): no current should show.
  • Continuity and polarity. With a test lamp (Wiring and Electrical Safety), check that the switch breaks the live, that live reaches the centre contact of every screw holder, and that earth is continuous to every metal case.
  • Insulators: the ink test on broken pieces, and no crackle or blue glow at night on line insulators in damp weather (Power Lines and Distribution).
  • Pull test. Tug each flex hard where it enters a fitting: the grip holds and nothing moves at the terminals.

Note Troubleshooting. A terminal or joint box is warm, or smells of hot rubber → a loose screw or a poor joint; switch off, cut back to clean copper, remake, and check again under load. Lamp flickers when the holder is touched → loose plunger spring or terminal, or a stranded end that has spread; refit. Line leaks in wet weather → cracked or porous insulators, or not enough sheds; replace with glazed ones with longer creepage paths. Rubber insulation has gone sticky or cracked → too hot, or untinned copper under it; replace the cable and find out why it got hot. Insulators crack after the first frost → underfired, porous porcelain; fire hotter, check with the ink test. Fuse blows when a lamp is screwed in → live and neutral swapped and the shell touching earthed metal, or a short in the holder; check polarity and spacing.

Dangers

Danger Electric shock and fire. Never work on a fitting that might be live. Switch off and remove the fuse, test with a known-working test lamp that the circuit is dead, then test the lamp again on a live circuit. Keep the fuse in your pocket so no one replaces it while you work. A badly made joint, terminal or lead can start a fire hours or days later, inside a wall or ceiling, at night. Never leave a joint twisted and taped without solder, never bury a joint box, and never cover a hot fitting. See Wiring and Electrical Safety for shock first aid.

  • High-voltage lines can kill without being touched: never work on insulators of a live line (Power Lines and Distribution).
  • Porcelain dust is fine silica: fettle and sweep wet.
  • Hot bitumen and solder burn deeply; heat bitumen slowly, keep water away, and keep a lid to smother it.
  • Lead sheath: wash hands after handling; never burn it (Lead).
  • Damaged leads are the commonest cause of workshop shocks: cut out the damaged length and remake it, never just tape it.

What this unlocks

With fittings, electric light and power can go safely into every house and workshop (Lamps and Candles, Electric Kettles, Irons, Heaters and Cookers, Fans, Vacuum Cleaners and Washing Machines) and out along the Power Lines and Distribution. The same porcelain skills make spark plugs (The Internal Combustion Engine), valve and tube bases (The Vacuum Tube), switchgear and heater parts; the jointing skills carry over to The Telephone and The Automatic Telephone Exchange cabling and to the Networks and the Internet of later chapters.

How it was first done

The first telegraph lines of the 1840s were strung on glass and glazed earthenware insulators, and threaded glass pin insulators that screwed onto a wooden pin were patented in the United States in the 1860s; by then porcelain makers in Britain and Germany were also making line insulators. As higher voltages came in around 1900, makers learned to fire thick porcelain completely and added more and longer sheds.

Inside buildings, Thomas Edison's system of 1880–82 brought the screw lamp cap and holder, fuses and junction boxes, while in Britain Joseph Swan's lamps were sold with the bayonet cap. Open "knob and tube" wiring on porcelain knobs and tubes was standard in North American houses from about 1880 to the 1930s, and the ceiling rose became a standard British fitting in the 1880s and 1890s. Charles Goodyear's vulcanised rubber (1844) gave the vulcanised-rubber cables of the late 1800s, made with tinned copper; plastic-insulated cables replaced rubber after the Second World War.

Source: content/entries/electricity/electrical-fittings.md