◆ Rebuild

Part 8 · Chemistry

Prussian Blue and the Prussiates

Prussian blue is the first modern synthetic pigment, a deep, strong, cheap blue made by mixing two iron salts in water. It colours oil paint, ink and blueprints, whitens laundry, tests for iron, and is the medicine that pulls radioactive caesium and poisonous thallium out of the body. This chapter makes the pigment from yellow prussiate and green vitriol, and tells honestly where the prussiate comes from and why it must never meet strong acid or fire.

Difficulty
●●●●●
Time
Two to three days to make, wash and dry a batch of pigment once you have yellow prussiate
Steps from zero
17 prerequisites →

You need first

Iron (the Bloomery)Pigments, Paints and Varnish

This unlocks

—
The full path from nothing — 17 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Simple Machines
  7. Hunting and Trapping
  8. Basic Woodworking
  9. Charcoal
  10. The Kiln
  11. Farming from Seed
  12. Hides and Leather
  13. Lime
  14. Oils and Pressing
  15. Bellows
  16. Pigments, Paints and Varnish
  17. Iron (the Bloomery)
  18. Prussian Blue and the Prussiates

Do them roughly in this order. See it on the tech tree →

Why it matters

Before 1704 a painter who wanted blue had two poor choices. Ground lapis lazuli (ultramarine) cost more than gold. Azurite and smalt were weak, greenish or grey. Prussian blue changed that. It is made from iron and a salt that a chemical works can produce by the tonne, it is so strong that a pinch tints a whole pot of white, and it is dark enough to stand in for black in shadows. Within forty years it was the standard blue of Europe, and within a century it was printing the Great Wave of Hokusai.

It does far more than colour pictures:

How it works

Iron forms two kinds of salt: ferrous (pale green, like green vitriol) and ferric (yellow-brown, like rust dissolved in acid). See Blueprints and Cyanotypes for more on the two.

Yellow prussiate of potash (potassium ferrocyanide) is a pale yellow crystal in which one iron atom is wrapped in a tight shell of six carbon–nitrogen groups. That shell is held so firmly that the salt is only mildly poisonous; it is even added in tiny amounts to table salt to stop it caking. When a solution of it meets ferric iron, the shells link up through the second kind of iron into an endless three-dimensional lattice, like a box of cubes. That lattice is Prussian blue. It does not dissolve in water, oil or weak acid. Its intense colour comes from electrons hopping between the two kinds of iron in the lattice.

Two properties matter for everything that follows:

  • Alkali destroys it. Lye, soda, lime or soap turn the blue to brown rust (ferric hydroxide) and set the yellow prussiate free again. So Prussian blue cannot be used in lime plaster, fresco or soap, and it can be recycled with lye.
  • The cubes have holes. Each cell of the lattice has a gap just the size of a caesium or thallium ion. In the gut, Prussian blue swaps its own loosely held potassium for these ions and holds them tight. That is why it works as an antidote.
Ferrous iron bonded to carbon Carbon Nitrogen each edge is one C≡N link Ferric iron bonded to nitrogen Trapped ion caesium or thallium held in the empty centre One cell of the lattice edge about half a millionth of a millimetre; the cells repeat in every direction iron at every corner, the two kinds alternating
Fig. 1 Inside Prussian blue. Iron atoms of two kinds sit at the corners of tiny cubes, joined along every edge by carbon–nitrogen links. The empty centre of each cube is just big enough to trap a caesium or thallium ion, which is how the pigment works as an antidote.

What you need

For one batch of about 7 g of pigment (scale up in proportion):

Item Amount Notes
Yellow prussiate of potash 10 g Pale lemon-yellow crystals. See below
Green vitriol (iron sulfate) 12 g Clean, pale green crystals, not rusty brown (Sulfuric Acid, Ink)
Nitric acid, or patience A few mL To turn the iron ferric (Nitric Acid); or let air do it (Method 2)
Rainwater or distilled water 3–4 litres Hard water spoils the colour and the washing
Glazed pots or glass jars, 1–2 L 3 No bare iron, copper, zinc or lead
Fine cloth filter, wooden paddle Tightly woven cotton or linen
Muller and glass or stone slab For grinding (Pigments, Paints and Varnish)

Where the prussiate comes from

Yellow prussiate is the hard part. It is not found in nature. Historically it has come from two places.

From gasworks waste (the better route). A gasworks cleans its gas by passing it through boxes of rusty iron ore (Coal and Coke). The ore takes out the rotten-egg sulfur gas and also traps cyanide compounds from the coal, turning them into Prussian blue inside the ore. After a few months this spent oxide is a lumpy mass, blackish and streaked with blue-green, with up to a tenth of its weight as iron–cyanide compounds. The works of the late 1800s recovered them like this:

  1. Break up the spent oxide and wash it with water to remove ammonia salts.
  2. Boil it with milk of lime (slaked lime stirred in water — Lime). The lime breaks down the Prussian blue in the ore and carries its prussiate into solution as a calcium salt. Filter.
  3. Stir in potash (Lye and Potash). Chalk falls out, and the liquid now holds potassium ferrocyanide. Filter again.
  4. Boil the liquid down and let it cool slowly. Lemon-yellow crystals of yellow prussiate grow, often several centimetres long. Recrystallise once from hot water.

No step uses acid or strong heat, and the cyanide stays locked in its iron shell throughout. Even so, treat spent oxide with care: it is full of sulfur, it can heat itself and smoulder when piled up fresh, and burning spent oxide gives off choking and poisonous fumes. Keep heaps small, damp and outdoors.

From animal waste (the old route, outline only). For its first 150 years yellow prussiate was made by fusing potash, scrap iron and charred blood, horn, hoof or leather at a red heat in iron pots, then leaching the cooled mass with water. The molten mass and its fumes contain free cyanide in deadly amounts, and a mistake while leaching it can release poison gas. This was dangerous work even for trained men in purpose-built works, and this book does not give working instructions for it. If your community has no gasworks, treat yellow prussiate as a chemical to make only once a proper chemical works with trained staff exists, or to obtain by trade.

Tip Recycle what you have. Prussian blue boiled with lye becomes brown rust plus yellow prussiate in solution. Filter off the rust and crystallise the yellow salt. Old blueprints, spoiled pigment and used laundry blue can all be recovered this way.

Method 1: The direct method (deep, insoluble blue)

1 Mix 2 Wash 3 Collect 4 Dry, grind prussiate stir blue at once fresh water blue settles blue mud muller dry in shade pour prussiate slowly into ferric iron solution settle, pour off clear water; repeat 5–6 times drain on tight cloth, then press between boards below 60 °C; grind in oil or gum on a slab
Fig. 2 Making Prussian blue. Yellow prussiate is poured slowly into ferric iron solution; a deep blue cloud forms at once. The blue is washed by letting it settle and pouring off the water several times, collected on a cloth, pressed, and dried in the shade before grinding.
  1. Make the iron solution. Dissolve 12 g of green vitriol in 150 mL of warm water with 3–4 drops of sulfuric acid. Add nitric acid a few drops at a time, warming gently, until the pale green turns to a clear yellow-brown; the iron is now ferric. This is the same step as in Blueprints and Cyanotypes. Work outdoors: brown fumes come off. Let it cool.
  2. Make the prussiate solution. Dissolve 10 g of yellow prussiate in 100 mL of water, cold or lukewarm. It dissolves easily to a pale yellow liquid.
  3. Mix: prussiate into iron. Pour the prussiate solution slowly into the iron solution, stirring all the time. A deep, inky blue forms at once. Pouring this way round keeps the iron in excess, which gives the insoluble blue, the kind that settles and washes well. (Pouring the other way gives the soluble kind; see Method 3.)
  4. Rest. Stir for 5 minutes more, then leave the jar for an hour. Fill it up with water, stir, and let it stand overnight.
  5. Wash by settling. The blue settles to the bottom as a soft mud. Pour off the clear water above it carefully. Fill with fresh water, stir, settle, pour off. Repeat five or six times, until the water above the blue tastes of nothing. Each wash takes several hours.
  6. Collect. Pour the blue mud onto a tightly woven cloth over a jar. Let it drain, then fold the cloth and press it gently between boards.
  7. Dry in the shade, at room temperature or a gentle warmth you can hold your hand in (below 60 °C). It dries to hard, dark lumps with a coppery sheen on the broken faces.
  8. Grind. Crush the lumps and grind them on the slab with a muller, first dry, then in the oil or gum you will use it in. Prussian blue is hard and grinds slowly.

Expect about 6–8 g of dry pigment.

Tip Keep some as paste. Dried Prussian blue becomes so hard that it never grinds as fine as the wet mud was. For watercolour and ink, keep part of the batch undried, as a thick paste in a closed jar with a drop of vinegar against mould.

Method 2: The air method (no nitric acid)

When you have no nitric acid, use the green ferrous salt directly and let the air finish the job.

  1. Dissolve 7 g of green vitriol in 100 mL of water with a teaspoon of vinegar, and 10 g of yellow prussiate in 100 mL of water.
  2. Pour the prussiate into the iron, stirring. A pale, whitish-blue mud forms. This is Berlin white, the same lattice with all its iron in the ferrous form.
  3. Pour the mud into a wide, shallow dish so it has plenty of air, and stir it several times a day. Over two to four days it turns steadily deeper blue as oxygen from the air changes the ferrous iron to ferric.
  4. When it no longer darkens, wash, collect and dry it as in Method 1.

This blue is a little lighter and redder in tone. Nineteenth-century works made their best grades, called Milori or Chinese blue, by this "indirect" route, using chemical oxidisers instead of air.

Method 3: Soluble blue for ink and laundry blue

Pour the iron solution slowly into the prussiate solution instead, using 7 g of green vitriol made ferric to 10 g of prussiate, so the prussiate stays in excess. The blue that forms holds extra potassium. Wash it two or three times by settling. As the salts wash out, it stops settling and begins to spread through the water as a clear deep-blue liquid. That is soluble Prussian blue: really a very fine suspension that passes through paper and cloth.

  • Blue ink. Stir 2 g of soluble blue paste into 50 mL of water with 1 g of gum arabic. It writes a clear, bright blue, does not corrode steel nibs, and is far more lightfast than plant blues (Ink, Pens, Nibs and Writing Instruments).
  • Laundry blue. Old linen and cotton yellow with age and washing. A trace of blue cancels the yellow, and the eye reads the result as white. Dilute the ink-strength blue (without gum) about ten times and store it in a bottle. Use one teaspoon (5 mL) per 10-litre bucket of the last, clean rinse, stir well, and swish the linen through it quickly so it takes the blue evenly.

Warning Rinse out all soap first. Soap, soda and lye destroy Prussian blue into rust. Blue added to soapy water leaves brown rust spots on the linen that are hard to remove. Add the blue only to clean, clear rinse water.

Using the pigment

Oil paint. Grind with about half its weight of linseed oil (Pigments, Paints and Varnish, Oils and Pressing). Prussian blue speeds the drying of oil, so it needs no drier. Used straight it is nearly black with a coppery sheen; it comes alive mixed with white. One part tints 20–50 parts of white to a clear sky blue. Mixed with yellow ochre it gives olive and leaf greens; with chrome yellow it gives the brilliant "chrome green" of carriages and railway engines (Chromium and Its Compounds).

Watercolour and printing ink. Grind the paste with gum arabic syrup for watercolour, or with boiled linseed varnish for printing ink (Printing). It prints a strong blue that does not bleed.

Where not to use it. Never in lime plaster, fresco, whitewash or casein paint made with lime; never on fresh concrete. The lime turns it brown within days.

Testing for iron. A drop of 5% yellow prussiate solution turns any liquid containing ferric iron blue. Add a drop of nitric acid first to make any ferrous iron ferric. Use it to find iron in well water (Water Treatment for a Town), to check ores (Finding and Identifying Ores), and on a scrap of cloth to test whether a stain is rust. Doctors use the same reaction (Perls' stain) to show iron deposits in thin slices of tissue under the The Microscope (Tissue Slides and the Microtome).

Prussian blue as an antidote

Caesium-137 is one of the main long-lived poisons released when a nuclear reactor is damaged (Nuclear Energy (Overview)). The body treats caesium like potassium and spreads it through all the soft tissues, and much of it is recycled through the bile and gut instead of being passed out. Thallium, a metal once common in rat poison, is handled the same way.

Prussian blue swallowed as a powder is not absorbed. It stays in the gut and traps caesium and thallium ions in its lattice as they pass through in the bile, so they leave in the faeces. It shortens the time caesium stays in the body by roughly two-thirds.

  • Dose used by doctors: adults 3 g three times a day; children of 2–12 years 1 g three times a day. It is usually continued for at least 30 days, guided by measuring radioactivity in the body or urine (Detecting Radiation).
  • Side effects: constipation, which must be treated because it slows the removal; blue-black faeces; and sometimes low blood potassium.
  • It does not help against radioactive iodine (use potassium iodide — Iodine), strontium, plutonium or uranium.

Warning For medicine, only the purest blue. Pigment for swallowing must be the insoluble kind of Method 1, made from clean crystals in glass or glazed vessels (never lead-glazed), washed until the wash water tastes of nothing, and dried without high heat. A doctor should decide whether to use it. It is a treatment for a real exposure, not a protective you take in advance.

How to tell it worked

  • Colour: deep blue in thin smears, nearly black in a mass; dried lumps show a coppery-bronze sheen on broken faces.
  • Vinegar test: a pinch in vinegar stays blue. A blue that fades or turns green is something else.
  • Lye test: a pinch in weak lye turns rust-brown within a minute. This is the surest sign of Prussian blue.
  • Insoluble or soluble: shake a pinch in clean water. Insoluble blue settles clear overnight; soluble blue stays as a blue liquid.
  • Strength: grind 1 part with 50 parts of white. Good Prussian blue still gives a definite clear blue.

Note Troubleshooting. Green or greenish-blue colour → some ferric hydroxide in the blue; the iron solution was not acid enough. Add a few more drops of acid to the iron next time, and rinse the blue in water with a splash of vinegar. The blue won't settle and runs through the filter → you made the soluble kind, or washed out all the salts. Add a little salt or a few drops of iron solution to make it settle, or use it as ink. Pale, whitish mud → the iron was still ferrous. Leave it in air and stir (Method 2), or add a little more ferric solution. Brown spots → alkali somewhere: hard water, a soapy pot or soda in the rinse. Gritty, weak paint → dried too hard or not ground long enough. Keep a paste for fine work.

Dangers

Danger Never mix the prussiates or Prussian blue with strong acids, and never heat them strongly, burn them, or throw them on a fire. Under those conditions they release cyanide gas, which kills in minutes. Keep prussiates on a separate shelf from acids, label them clearly, and pour used solutions onto waste ground away from water, never into a drain where acid may be. Weak, cold acids such as the few drops of sulfuric acid, vinegar or nitric acid in this chapter are safe because the prussiate is never heated with them. Do not change the recipes to use more acid or heat.

  • Yellow prussiate itself is only mildly poisonous, but do not eat it. Wash hands after handling.
  • The animal-waste fusion that makes yellow prussiate from blood and horn produces free cyanide. It is for a proper chemical works only.
  • Spent oxide can self-heat and smoulder, giving off sulfur dioxide and other poisonous fumes. Keep it damp and in small heaps outdoors.
  • Nitric acid fumes in Method 1 are poisonous: work outdoors (Nitric Acid).
  • Prussian blue pigment is not poisonous: it is a medicine. Still, avoid breathing its dust.

What this unlocks

How it was first done

In Berlin around 1704–1706 the paint-maker Johann Jacob Diesbach was making a red lake from cochineal, iron sulfate and alum, using potash. He had borrowed the potash from the alchemist Johann Konrad Dippel, and it was contaminated with Dippel's "animal oil", distilled from blood. Instead of red, Diesbach got a deep blue. The new "Berlin blue" was announced in 1710, its recipe kept secret until the Englishman John Woodward published it in 1724. It spread rapidly through Europe; Antoine Watteau, Canaletto and Gainsborough all used it.

In 1752 the French chemist Pierre-Joseph Macquer showed that alkali breaks Prussian blue into iron oxide and a soluble yellow substance, the start of the chemistry of the prussiates. Prussian blue reached Japan as bero-ai ("Berlin indigo") and from the late 1820s transformed woodblock printing; Katsushika Hokusai's Great Wave off Kanagawa (about 1831) is printed largely in it.

From the 1840s Sir John Herschel's cyanotype (Blueprints and Cyanotypes) put Prussian blue in every drawing office. Gasworks spent oxide replaced animal waste as the main source of prussiates late in the 1800s. Its use as an antidote was developed from the 1960s; after the Goiânia accident in Brazil in 1987, when a Radiotherapy (Overview) source scavenged from an abandoned clinic spread caesium-137 through a city, Prussian blue was given to dozens of contaminated people, and it has been stockpiled as a radiation countermeasure ever since.

Source: content/entries/chemistry/prussian-blue.md