◆ Rebuild

Part 3 · Metals

Nickel and Cobalt

Two hard, silvery, magnetic metals that hide in green, pink and bronze-coloured ores. Cobalt was used for thousands of years only as a blue colour; nickel was called the "devil's copper" because it spoiled copper smelts. Learned properly, they give white coinage alloys, rust-proof plating, tough steels, heating wire, magnets and batteries.

Difficulty
●●●●●
Time
A day to sort and test ore; weeks for a matte smelt and convert; months to set up an electrolytic refinery
Steps from zero
16 prerequisites →

You need first

Finding and Identifying OresCharcoalElectrolysis

This unlocks

Electric Kettles, Irons, Heaters and CookersPermanent Magnets
The full path from nothing — 16 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Salt
  12. Fermentation
  13. Bellows
  14. Copper Smelting
  15. The Battery
  16. Electrolysis
  17. Nickel and Cobalt

Do them roughly in this order. See it on the tech tree →

Why it matters

Nickel and cobalt sit next to iron in the table of elements, and they behave like its tougher, cleaner cousins. Both are hard, silvery-grey, take a high polish, resist rust far better than iron, and — like iron — stick to a magnet. Small amounts change other metals completely:

  • Nickel whitens copper into cupronickel (coins, condenser tubes, ships' pipes) and, with zinc, into nickel silver, a cheap white metal for spoons, instrument parts and keys. It toughens steel and, with chromium, makes stainless steel (Alloy and Stainless Steels). A thin skin of it stops iron rusting (Electroplating). Nickel with 20% chromium is nichrome, the wire inside every electric heater, toaster and small furnace. Nickel hydroxide is the positive plate of the nearly indestructible nickel-iron battery (The Rechargeable Battery). Nickel-coated wire and sheet make the insides of a The Vacuum Tube.
  • Cobalt in a pinch colours glass, glaze and enamel deep blue (Glazes, Enamel on Metal). It makes the strongest permanent magnets before modern rare-earth ones (Permanent Magnets), the hardest-wearing cutting alloys, and the paint "drier" that makes linseed oil paint set overnight (Pigments, Paints and Varnish).

Be honest about where this sits. Copper, iron and tin come first and are far easier. Nickel and cobalt are for a community that already smelts copper, has a crucible furnace reaching 1,400 °C (Firebrick and Refractories) and a supply of direct current (The Generator, Electrolysis). The cobalt blue route is the exception: it needs only a roasting fire and glass, and has been done since the Bronze Age.

How it works

Nickel and cobalt rarely occur as their own ore. They hide inside three kinds of rock:

  1. Sulfide ores — nickel and iron combined with sulfur (pentlandite), usually mixed with lots of magnetic iron sulfide (pyrrhotite) and copper ore. This is the world's main nickel source.
  2. Laterites — deep red tropical soils over a green rock called serpentine. Rain has leached everything else away and left nickel behind, sometimes concentrated in bright green crusts (garnierite). They are smelted to ferronickel (Alloy and Stainless Steels) or dissolved in hot acid under pressure (Leaching, Solvent Extraction and Electrowinning).
  3. Arsenide ores — nickel and cobalt combined with arsenic, in silver and copper veins. They gave the metals their names and their bad reputation. They are poisonous to roast; see Arsenic.

The basic trick for sulfide ores is the one used for copper: matte smelting. Melt the ore with sand. Iron combines with oxygen and the sand into a light, glassy slag that floats; nickel, copper and cobalt stay with the sulfur in a heavy, metallic-looking liquid called matte that sinks. Blow air through the matte and more iron and sulfur burn away, until you have a matte of nearly pure nickel-copper sulfide. Roast that to oxide, reduce it with charcoal, and you get a copper-nickel alloy directly.

Getting pure nickel is harder, because nickel and copper are so alike. The reliable modern route is electrolytic refining: cast impure nickel into plates, hang them in a warm nickel sulfate solution, and pass a current. Nickel dissolves from the impure plate and is laid down, pure, on a thin starting sheet (Electrolysis). Faraday's law gives 1.09 g of nickel per ampere-hour, the same figure as for nickel plating.

Where to find it

Three kinds of ore Sulfide ore bronze pyrrhotite (pulled by a lodestone) with paler pentlandite and brassy copper ore; dark host rock Laterite deep red tropical soil; bright apple-green garnierite crusts and veins just above the green-black serpentine rock Arsenide vein tin-white heavy ore that smells of garlic; pink cobalt bloom and green nickel bloom. Means arsenic: deadly smoke The borax bead test a glass bead of melted borax on a wire loop, touched to a speck of roasted ore and remelted Cobaltdeep pure blue Nickelbrown; grey inthe smoky flame Ironyellow tobottle-green Coppergreen-blue
Fig. 1 Recognising nickel and cobalt ores. Sulfide ore is bronze-coloured and magnetic; laterite carries bright green garnierite; arsenide veins weather to green "nickel bloom" and pink "cobalt bloom". The borax bead test tells the two metals apart.
Sign What it is Notes
Heavy bronze-yellow to brown metallic ore that a lodestone pulls Pyrrhotite, with paler, non-magnetic grains of pentlandite and brassy chalcopyrite Dark rock (gabbro, norite) in old shield country. The Sudbury basin in Canada and Norilsk in Siberia are giant examples. Weathers to a rusty gossan (Finding and Identifying Ores)
Apple-green to emerald-green soft crusts, veins and earthy lumps Garnierite in laterite Red, deeply weathered soils over greasy, green-black serpentine rock in hot, wet lands: New Caledonia, Cuba, Indonesia, the Philippines, Brazil. Easiest nickel ore to find, but low grade (1–3% nickel)
Pale copper-red metallic ore that is not copper Nickeline (nickel arsenide, kupfernickel) In silver-cobalt veins. Smells of garlic when struck or heated
Tin-white to steel-grey heavy metallic grains Cobalt and nickel arsenides (skutterudite, cobaltite) Same veins. Garlic smell when struck hard with steel
Pink, peach or purple crusts and tiny needles Erythrite, "cobalt bloom" The best field sign of cobalt below. Means arsenic too
Pale apple-green powdery crusts on arsenide ore Annabergite, "nickel bloom" Means nickel, and arsenic
Iron meteorites Iron with 5–10% nickel Heavy, magnetic, rusty, with a thin black crust. Rare but real

Tests with no laboratory.

  • Borax bead. Melt a little borax into a clear glass bead on a loop of iron or platinum wire in a hot flame, touch it to a speck of roasted ore powder, and melt again (Identifying Substances). Cobalt gives a deep, pure blue — a speck too small to see is enough. Nickel gives a brown to red-brown bead in the hot, outer part of the flame, turning grey and cloudy in the inner, smoky part. Iron gives yellow to bottle-green; copper gives green-blue.
  • Colour of the solution. Roast a pinch of ore, then warm it in dilute Hydrochloric Acid or Sulfuric Acid. Nickel gives a clear green liquid; cobalt a pink to rose-red one. Add ammonia water (Ammonia) drop by drop: nickel solution turns deep blue-violet.
  • Cobalt's colour change. Paint a little pink cobalt chloride solution on paper and dry it over the fire. It turns blue when dry and back to pink in damp air. This proves cobalt — and makes a useful damp-indicator for stores and instruments.

What you need

Item Amount Notes
Sorted sulfide ore 50–200 kg per smelt Hand-picked and crushed to walnut size; the richer the better
Quartz sand About a quarter of the ore weight Flux to make the iron slag. Adjust by trial
Limestone A tenth of the ore weight Makes the slag runnier
Charcoal or coke About the ore weight Charcoal, Coal and Coke
Furnace Clay-lined shaft furnace or reverberatory furnace with a strong blast As for copper matte smelting (Copper Smelting, Firebrick and Refractories)
Converter Clay- or silica-lined pot with tuyeres, or a bigger tuyere and a strong blast in a deep hearth Steel in Quantity describes converters
Crucibles Graphite-clay, good to 1,450 °C For alloys (Firebrick and Refractories)
Electrolytic tanks Wood lined with pitch, or stoneware, 100–400 litres Electrolysis
DC supply 2–3 V per tank, tens to hundreds of amperes The Generator

Method 1: Cobalt blue (zaffre and smalt)

This is the oldest use and the one to try first. A few grams of cobalt colour kilograms of glass.

  1. Pick the ore. Choose pieces with pink bloom or grey arsenide, and crush them to sand size.
  2. Roast outdoors, upwind, far from houses, wells and fields, in a shallow iron pan or on a stone hearth over a wood fire. Stir from a distance with a long rake. A white smoke with a strong garlic smell pours off: that is arsenic oxide, a deadly poison (see Dangers and Arsenic). Roast at a dull red heat (600–700 °C) until no more white smoke comes, often 6–12 hours. What remains is dark grey-black cobalt oxide with some iron and nickel.
  3. Zaffre. Grind the roasted ore and mix it with two to three parts of fine quartz sand. This is zaffre, sold for centuries to glassmakers and potters. Use ¼–1% in a glaze for a strong blue (Glazes).
  4. Smalt. Melt one part roasted cobalt ore with about three parts quartz sand and two parts potash (Lye and Potash, Glass) in a crucible. Nickel and iron, being heavier, collect at the bottom as a metallic button called speiss — keep it, it is a nickel ore. Pour the deep blue glass into water to shatter it, grind it wet, and settle it in tubs: the coarse grains, which sink first, are the deepest blue. Smalt was the blue paint pigment of Europe for three centuries (Pigments, Paints and Varnish).
  5. A brighter blue (Thénard's blue, 1802): dissolve the roasted cobalt in acid, mix the pink solution with a solution of alum, add Lye and Potash or soda solution to throw down a mixed precipitate, wash it, dry it, and heat it bright red for an hour. You get cobalt aluminate, a clean, brilliant blue that does not fade.

Method 2: Matte smelting sulfide ore

1 Partial roast burn off a third of the sulfur 2 Smelt slag floats, heavy matte sinks 3 Convert blow air: iron burns into the slag 4a Roast, reduce with charcoal at 1,400 °C: copper–nickel alloy (Monel, cupronickel) 4b Crude nickel cast into anodes, refined in the cell below The refining cell + − Clean solution fed in level inside bag 2–3 cm higher Crude nickel anode (+) dissolves slowly Cathode (−) in canvas bag liquid seeps outward, so dirty liquid never reaches the cathode Pure nickel grows here 50–60 °C, 1.5–2 A/dm², 2–3 V Anode sludge sulfur, copper, precious metals
Fig. 2 From ore to metal. Sulfide ore is smelted to matte, the iron is blown out as slag in the converter, and the nickel-copper matte is either roasted and reduced straight to a copper-nickel alloy, or cast into anodes and refined to pure nickel in a cell where each cathode hangs in a cloth bag.
  1. Partial roast. Spread the crushed ore in heaps on a bed of wood and burn it slowly for several days, as for copper sulfide ore (Copper Smelting). Burn off only about a third of the sulfur: the ore turns from bronze to dull brown on the outside but stays bright inside when broken. Roasting releases sulfur dioxide — a choking gas. Do it well away from people, or catch it for Sulfuric Acid.
  2. Smelt. Charge the furnace with layers of fuel and a mixture of roasted ore, quartz sand and a little limestone. At a bright yellow heat (1,200–1,300 °C) everything melts. Tap the furnace: a black glassy slag runs off the top, and a heavy, dull bronze-grey matte runs from a lower tap hole or is ladled from the bottom. A first smelt might turn ore with 2% nickel into matte with 10–20%.
  3. Convert. Melt the matte again (or keep it molten) in a lined converter and blow air through it with quartz sand added. The iron sulfide burns first: the iron goes into the slag, the sulfur leaves as gas, and the bath stays hot from its own burning. Skim the slag often. Stop when the flame shortens and the slag carries little iron — before the nickel itself starts to oxidise into the slag. The result, called Bessemer matte, is about three-quarters nickel and copper and a fifth sulfur, with almost no iron.
  4. Dead roast. Crush the converted matte fine and roast it at red heat (700–900 °C) with frequent stirring until it no longer smells of sulfur, for a day or more. It becomes a dark grey-green oxide powder.
  5. Reduce to alloy. Mix the oxide with a quarter of its weight of powdered charcoal and a little borax, pack it into a covered graphite-clay crucible, and heat it to white heat (about 1,400 °C) for one to two hours. A silvery copper-nickel button forms. If the ore had roughly twice as much nickel as copper, as at Sudbury, the button is close to Monel: about two-thirds nickel, one-third copper — tough, bright, nearly rustproof, and excellent for pump parts, valves and salt-water fittings.

If your ore has more copper than nickel, add copper to bring it to 75 copper : 25 nickel (cupronickel, the classic white coin metal), or add zinc as well for nickel silver (below).

Method 3: Electrolytic nickel

For pure nickel — for plating anodes, battery plates, vacuum tubes and nichrome — you must separate it from copper, iron and cobalt. This is chemistry work and takes practice; read Electrolysis first.

  1. Make crude nickel. Roast the converted matte to oxide as above. Soak the powder in warm dilute Sulfuric Acid (about 1 part acid to 10 of water) for a day, stirring: much of the copper dissolves, giving blue copper sulfate (save it for Electroplating). Wash the residue, mix it with charcoal, and reduce it in a crucible as in Method 2 to a crude nickel that still has some copper, iron and cobalt. Cast it into flat anodes, about 1–2 cm thick and the size of a book page.
  2. Make the bath. Dissolve nickel in warm sulfuric acid to make a green nickel sulfate solution, with about 60–80 g of nickel per litre. Add a little salt (for chloride, which helps the anodes dissolve evenly) and about 15 g per litre of boric acid (made from borax and acid, see Borax and Boric Acid) to steady the acidity.
  3. Purify the bath — the whole secret. Impurities in the solution will plate out with the nickel, so clean it continuously:
    • Iron: bubble air through the warm solution, or add a little Chlorine and Bleach, and stir in nickel carbonate or a little Lime water until it is only faintly acid (just enough to turn blue litmus barely red, about pH 5). Rust-brown iron hydroxide settles. Filter.
    • Copper: stir in nickel scrap or powder for a few hours. Copper is laid down on it as red powder. Filter.
    • Cobalt: add bleach a little at a time at the same mild acidity, stirring. Cobalt is oxidised before nickel and comes down first as a black precipitate. After each addition, filter a spoonful and borax-bead the solid: stop when the bead shows nickel's brown as well as cobalt's blue. The split is never perfect; repeat it on the black solid if you want purer cobalt. Save that solid — it is your cobalt.
  4. The cell. In a pitch-lined wooden tank, hang the crude nickel anodes. Between them hang cathodes, each inside a bag of tight canvas stretched on a wooden frame (a diaphragm). Feed the clean solution into the bags, so the liquid level inside each bag stays 2–3 cm higher than outside. The clean liquid always seeps outward through the cloth, so the dirty liquid round the anodes never reaches the cathode.
  5. Starter sheets. Plate nickel for a day onto polished steel sheets lightly rubbed with tallow, peel the thin nickel skin off, and use these as the cathodes.
  6. Run it. Keep the bath at 50–60 °C (too hot to keep a hand in for more than a few seconds), with 1.5–2 A for every square decimetre of cathode, at 2–3 V per tank. A cathode of 1 m² (both faces counted) at 2 A/dm² takes 200 A and gains about 5 kg of nickel a day. Lift the cathodes after one to two weeks.
  7. Clean the anode sludge. The crude anodes leave a black sludge in the tank bottom containing sulfur, copper and any precious metals (Gold and Silver). Collect it whenever you change anodes.

Alloys and products

Alloy Recipe (by weight) Melts about Uses
Cupronickel 75 Cu, 25 Ni (or 70/30, 90/10) 1,200–1,250 °C Coins, salt-water pipes, condenser tubes and heat exchangers in ships (Metal Pipes and Tubes)
Nickel silver (German silver) 60 Cu, 20 Ni, 20 Zn (10–30 Ni) about 1,100 °C Spoons and forks (plated as "EPNS" with silver), keys, instrument parts, springs, zips
Monel 67 Ni, 30 Cu, a little iron and manganese about 1,330 °C Pumps, valves, propeller shafts, acid-resistant parts
Nichrome 80 Ni, 20 Cr about 1,400 °C Heating wire for stoves, kilns, soldering irons and lab furnaces; does not burn through at bright red
Invar 64 Fe, 36 Ni — Barely expands with heat: clock pendulums, measuring tapes (Measurement from Scratch)
Alnico Iron with 8–12 Al, 15–26 Ni, 5–24 Co, some Cu — Cast permanent magnets (Permanent Magnets, The Electric Motor, The Telephone)
Stellite Cobalt with about 30 Cr, 4–13 W, 1–3 C — Hard-facing valve seats and cutting edges; holds its edge at red heat

Making nickel silver. Melt the copper first in a crucible under a charcoal cover. Add the nickel (as small pieces of cupronickel or crude nickel, which dissolve into the copper at far below nickel's own melting point of 1,455 °C). Stir with a dry clay or graphite rod. Pull the crucible slightly back from the hottest fire, let it cool to orange, and only then push in the zinc, warmed, under the charcoal — zinc boils at 907 °C and will flare and fume away if added too hot (Zinc and Brass). Stir and pour into ingot moulds (Metal Casting). Roll or draw it like brass (Sheet Metal and Rolling, Iron and Brass Wire); anneal it often, at a dull red.

Nickel plating is in Electroplating. Nickel's own melting point (1,455 °C) and toughness make it harder to cast and forge than copper, so pure nickel is best used as plating anodes, electrolytic sheet, or powder.

How to tell it worked

  • Magnet. Pure nickel and cobalt are both attracted to a magnet; cupronickel and nickel silver are not (they look like silver but a magnet ignores them). If a "nickel" sample is strongly magnetic and rusts in a week of damp air, it is mostly iron.
  • Colour and tarnish. Nickel is greyish-white with a faint warm tint, cobalt slightly bluish-grey. Both stay bright in damp air for months where iron would rust in days.
  • Solution test. A filing dissolved in warm acid gives green (nickel) or pink (cobalt) liquid. Dip a bright iron nail in your nickel sulfate solution for a minute: it should come out unchanged. A copper-red film on the nail means copper is still there.
  • Cathode quality. Good electrolytic nickel is smooth, grey-white, tough and bends before it breaks.

Note Troubleshooting. Matte will not separate from slag; everything is one sticky mass → too little quartz sand, or too cool. Add sand and fuel, and blow harder. Converter freezes → you blew too long and burned the iron that was keeping it hot, or the charge was too small. Convert larger batches, add fresh matte, and stop sooner. Alloy button full of holes or crumbly → oxide not fully reduced, or sulfur still in it. Roast longer until there is no sulfur smell; use more charcoal and a longer, hotter melt. Cathode dark, rough and brittle, with "trees" growing on it → solution dirty (copper, iron), too little boric acid, or too much current. Purify again, lower the current, check the bag level. Cathode peels and curls → stress from too high a current, or too cold a bath. Warm it to 50–60 °C. Pitted cathode → hydrogen bubbles clinging. The bath is too acid; raise it toward pH 5 with nickel carbonate, and rock the cathodes gently. Smalt is pale or grey → too little cobalt or too much iron. Hand-pick better ore, and let the speiss settle out longer.

Dangers

Danger Arsenic. Cobalt and many nickel ores carry arsenic. Roasting them releases arsenic oxide, a white, garlic-smelling smoke that kills by poisoning slowly or quickly, and settles on crops, pasture and water downwind. Roast only outdoors, upwind of everything, far from wells, with your face covered and your clothes washed afterwards. Never let children or animals near the roasting ground or its dust. Read Arsenic before you begin.

Danger Nickel carbonyl. Modern refineries purify nickel by passing carbon monoxide over warm nickel powder, making a gas, nickel carbonyl, that is then broken down again. It is one of the most poisonous gases known: a lungful you cannot even smell can kill a few days later. Do not attempt it. Do not heat fine nickel powder in charcoal fumes in a closed space.

  • Sulfur dioxide from roasting and converting burns the lungs and kills plants downwind. See Sulfuric Acid.
  • Nickel allergy. Many people come out in an itchy rash where nickel touches their skin. Workers with nickel salts get "nickel itch". Wash, wear leather gloves, and keep nickel off jewellery and buttons for those affected.
  • Cancer and lungs. Breathing nickel dust and roasting fumes for years causes cancers of the nose and lungs; breathing cobalt dust causes a scarring lung disease. Work wet, ventilate, and cover your mouth and nose with wet cloth.
  • Cobalt in food. Cobalt salts are poisonous to the heart in any but tiny amounts. In the 1960s, brewers in Quebec and elsewhere added cobalt to beer to improve its foam, and dozens of heavy drinkers died of heart failure. Never use cobalt compounds near food.
  • Molten metal, hot acid and electricity — see Metal Casting, Acids, Bases and Testing and Electrolysis.

What this unlocks

Pure nickel and its salts for Electroplating and the nickel-iron cell (The Rechargeable Battery). Nickel steels and stainless (Alloy and Stainless Steels). Nichrome heating wire for electric kilns, ovens and laboratory furnaces. White, durable coinage (Money, Trade and Record-keeping). Cobalt blue for Glazes, Glass, Enamel on Metal and Pigments, Paints and Varnish. Alnico magnets for better The Electric Motors, The Generators, The Telephone receivers and loudspeakers. Nickel catalysts harden plant oils into solid fats (Oils and Pressing, Soap).

How it was first done

Cobalt blue glass and glaze go back to Egypt and Mesopotamia in the second millennium BC; cobalt was the blue of Chinese blue-and-white porcelain from the 1300s, and Persian ore was traded across Asia for it. The Chinese also made paktong ("white copper"), a copper-nickel-zinc alloy, from the ores of Yunnan, probably by the 1500s or earlier; it was exported to Europe in the 1700s. In the silver mines of the Ore Mountains of Saxony, miners blamed goblins (kobolds) for ores that gave off poisonous smoke and no silver, and a red ore that looked like copper but gave none was called kupfernickel, "copper-devil". Saxon works made zaffre and smalt from these ores from the 1500s.

The Swedish chemist Georg Brandt showed around 1735 that the blue came from a new metal, cobalt. His countryman Axel Fredrik Cronstedt isolated nickel from kupfernickel in 1751. In the 1820s German makers, notably in Berlin and Saxony, copied paktong as "German silver". Nickel coins came in the 1850s–60s (the American five-cent "nickel" of 1866 is still 75% copper, 25% nickel). The giant nickel ores of New Caledonia were found by Jules Garnier in 1864 and those of Sudbury, Canada, during railway building in 1883. Ludwig Mond invented the carbonyl process in 1890; Monel was named in 1906; and electrolytic refining with bagged cathodes was developed by Noak Victor Hybinette in Norway in the early 1900s.

Source: content/entries/metals/nickel-and-cobalt.md