◆ Rebuild

Part 5 · Cloth and Clothing

Blankets, Curtains, Rugs and Towels

The cloth things that make a house warm and comfortable — raised wool blankets, sheets, pillowcases and duvets, curtains with their rods and blinds, woven, knotted, braided and rag rugs and carpets, mats and doormats, cushions, terry towels and handkerchiefs — how to weave and sew each, and what size to make it.

Difficulty
●●●●●
Time
A blanket woven in 2–4 days and raised in an afternoon; sheets and curtains a day each to sew; a rag rug in 2–3 days; a knotted pile rug a month or more
Steps from zero
6 prerequisites →

You need first

The LoomSewing, Needles and Thread

This unlocks

—
The full path from nothing — 6 steps before this one
  1. Cordage and Rope
  2. Stone Tools
  3. Basic Woodworking
  4. Spinning and Weaving Cloth
  5. The Loom
  6. Sewing, Needles and Thread
  7. Blankets, Curtains, Rugs and Towels

Do them roughly in this order. See it on the tech tree →

Why it matters

Soft furnishings keep heat in, keep draughts and light out, protect floors, and make a house pleasant to live in. They also matter for health: clean bedding and towels, washed hot, cut down lice, fleas, scabies and skin infections (Personal Hygiene, Laundry and Bleaching Cloth).

Almost all of them are plain cloth from the The Loom, cut and hemmed (Sewing, Needles and Thread). What is particular to each — the size, the weave, the finishing — is in this chapter. Quilts and down are in Quilting, Down and Warm Clothing, mattresses and pillows in Mattresses and Upholstery, felt rugs in Felt, plaited rush mats in Baskets and Containers, and oiled floorcloths in Linoleum, Oilcloth and Floorcloths.

How it works

  • Warmth is still air. A blanket is warm because it holds a layer of still air. A raised (brushed) surface — fibre ends teased up into a soft fuzz called the nap — traps far more air than flat cloth of the same weight.
  • Absorbing water needs surface. A towel dries you by sucking water into its fibres. Loops of yarn standing up from the cloth (terry) give many times more surface than flat cloth. Cotton and linen soak up water well; linen also dries fast.
  • Pile takes the wear. In a pile rug or carpet the yarn ends stand on end, so feet wear the tips, not the woven foundation beneath. Denser pile lasts longer.
  • Curtains stop a cold air current. A window chills the air next to it, which sinks and spreads across the floor. Heavy, lined curtains reaching the floor, under a closed top (a pelmet or a board), trap that air behind them. Well fitted, they can cut the heat lost through a window by a quarter or more.

What you need

Item For Notes
Wool yarn, medium, woollen-spun Blankets, rug pile, rug weft Wool, The Spinning Wheel
Linen or cotton yarn, fine and strong Sheets, towels, handkerchiefs, rug warps Flax, Hemp and Linen, Cotton
Floor loom, 90–120 cm wide Most weaving The Loom; a warp-weighted loom for wide blankets (Spinning and Weaving Cloth)
Upright rug loom Pile rugs Two heavy beams in a strong frame (below)
Teasels Raising blankets Dried seed heads of fuller's teasel
Old cloth Rag and braided rugs Any worn clothing or bedding
Down, feathers, kapok, wool Duvets, cushions Quilting, Down and Warm Clothing
Hardwood Curtain rods, rollers Ash, beech or any straight hardwood (Basic Woodworking, The Lathe)
Coir, rush or rope Doormats Coconut husk fibre (Cordage and Rope); rush; old rope

Fuller's teasel is a tall plant with egg-shaped seed heads covered in stiff hooked bracts; cut the heads in late summer when brown, and dry them. Wild teasel, with straight spines, is weaker but usable.

Blankets

A blanket is a soft, thick wool cloth, woven a little open, fulled to thicken it, then raised.

  1. Size. Finished: single bed 180 × 230 cm; double bed 230 × 250 cm. Weave about 15% wider and longer to allow for shrinkage in fulling. On a loom narrower than the blanket, weave two lengths and sew them edge to edge down the middle with a flat butted seam (Sewing, Needles and Thread).
  2. Yarn. Soft, woollen-spun singles about 1.5–2 mm thick, spun loosely so the fibres can be drawn out into nap. Fine short wool is best.
  3. Weave a 2/2 twill (each weft passes over two warps and under two, stepping one thread each row, The Loom), at about 5 threads per cm each way. Twill packs more yarn than plain weave and raises better. Beat lightly: the cloth should look a little open on the loom.
  4. Full it gently in warm soapy water, squeezing and pounding until it has shrunk 10–15% and the weave has closed into a soft, firm cloth (Felt, Spinning and Weaving Cloth). Rinse.
  5. Raise while it is still damp. Mount 10–20 teasel heads side by side in a wooden frame with a handle (a "teasel handle"). Lay the blanket over a smooth pole or a sloping board. Draw the teasels firmly along the warp in one direction only, in long strokes, so the hooks catch fibre ends and pull them out of the yarn. Work over the whole surface, then turn the cloth over and do the other side. Several light passes are better than one heavy one: dig in hard and you tear the cloth.
  6. Finish. Dry it stretched on a frame or pegged out flat, nap all lying one way. Bind the cut ends with blanket stitch or a strip of tape; the woven selvedges need nothing.
RAISING A BLANKET pole teasel handle one way, along the warp damp, fulled wool nap fibre ends pulled up THREE-PICK TERRY 1. Picks 1 and 2 beaten short of the cloth picks 1 and 2 pile warp, slack ground warp, tight gap 5–10 mm reed 2. Pick 3 beaten home: all three slide up and the slack pile warp buckles into a loop loop (the next setloops to the back)
Fig. 1 Raising a blanket and weaving terry. Teasels drawn along damp, fulled wool pull fibre ends up into a warm nap. In terry, a slack pile warp is pushed up into loops when the third weft pick drives two loosely placed picks up to the cloth.

A water-powered gig mill is a drum covered with teasels turning against cloth drawn past it (The Watermill); later machines used wire card clothing (Textile Machinery).

A good blanket weighs 1.5–2.5 kg for a single bed, holds up against the light as an even glow with no thin patches or holes, has a nap 2–5 mm deep that springs back when pressed, and does not shed loose fibres in your hand.

Sheets and pillowcases

Sheets are plain-weave linen or cotton, 15–25 threads per cm (Spinning and Weaving Cloth), bleached in the sun (Laundry and Bleaching Cloth).

  • Sizes: single bed 180 × 260 cm; double 230 × 260 cm — long enough to tuck in 25–30 cm at the sides and foot.
  • Narrow looms: weave two widths and join them down the centre with a flat seam. When the middle wears thin — it always wears first — cut the sheet down the centre, sew the two old selvedges together, and hem the new outer edges. This sides-to-middle trick doubles the life of a sheet.
  • Hems: 1–1.5 cm at the sides (none on selvedges), 5–7 cm at the top so you can tell the head end, 2–3 cm at the foot.

Pillowcase for a pillow 50 × 75 cm (Mattresses and Upholstery):

  1. Cut a strip of the same cloth 53 cm × 176 cm (75 + 75 for front and back, 15 for an inner flap, and about 11 cm for hems).
  2. Hem both short ends: 1 cm on one, 4–5 cm on the other (the open end).
  3. Fold the narrow-hemmed end over by 15 cm to make the flap. Then fold the wide-hemmed end back over it until the case is 75 cm long, faces together.
  4. Sew both long sides through all layers, 1.5 cm in, with a French seam (Sewing, Needles and Thread). Turn it right side out. The flap tucks over the end of the pillow and needs no buttons.

Duvets and covers

A duvet (or continental quilt) is a flat bag of down or feathers that lies loose on top of the sleeper inside a washable cover. It replaces several blankets.

  1. Size: single 135 × 200 cm; double 200 × 200 cm.
  2. Ticking: very tightly woven cotton or linen, 40 threads per cm or more, so down cannot work out. Rubbing beeswax into the inside face helps a looser cloth.
  3. Channels: sew the top and bottom layers into channels or squares 20–30 cm across, using walls of light cloth (baffles) for the warmest duvets or sewing straight through for lighter ones (Tents, Sleeping Bags and Camping Gear shows the difference). Without channels, the down drifts to the edges.
  4. Fill: each compartment with its share of washed down (Quilting, Down and Warm Clothing). A single winter duvet takes about 500–900 g of good down; feather alone needs about twice that weight.

Duvet cover: a bag of sheeting 3 cm bigger than the duvet each way, open along the foot end with 5–6 buttons or ties (Buttons, Buckles, Hooks and Zips), and with a cloth tie sewn inside each corner to tie to loops on the duvet so it does not bunch up.

Curtains, rods and blinds

CURTAINS ON A ROD finial 10–15 cm 15–25 cm curtain 2 × rod width, lined hem 1 cm above the floor SPRING ROLLER BLIND flat pin coil spring inside roller ratchet pull down: winds spring stiffened cloth pull ring pawl drops into a notch when the blind is still
Fig. 2 A lined curtain on a rod, and a roller blind. The rod is fixed above the window and extends beyond it on each side so the drawn curtains clear the glass. The roller blind's spring inside the roller winds it up; a pawl catching a ratchet holds it where it stops.

Curtains

  1. Width: 1.5–2.5 times the width of the rod, so the curtain hangs in deep folds even when drawn shut. Twice is usual. Divide between two curtains that meet in the middle.
  2. Length: to just above the sill (1 cm) for a small window, or to 1 cm above the floor for warmth. Add 15–20 cm for top and bottom hems.
  3. Cloth: any close-woven cloth. For warmth, add a lining of cotton or linen, and between them an interlining of flannel or an old blanket. The lining also protects the cloth from sun.
  4. Side hems: fold 3–4 cm twice and hem. Bottom hem: fold 8–10 cm twice; put a few small weights in the corners (lead discs, pebbles in pockets, or a light chain along the hem) so it hangs straight.
  5. Top: fold over a 6–8 cm casing to slide straight onto the rod; or sew on rings of wood or brass every 12–15 cm; or loops of tape.
  6. Lining: cut it 5 cm narrower and shorter, sew it face-to-face down the sides, turn, and hem the bottoms separately.

Curtain rod: a straight hardwood pole 25–35 mm thick, turned or planed round, with a finial (knob) at each end so the rings cannot slide off. Fix it 10–15 cm above the window frame on brackets of wood or forged iron (Blacksmithing), extending 15–25 cm beyond the frame on each side. For light curtains, an iron rod 10–12 mm thick (Iron and Brass Wire) is enough. Rings slide better on a waxed pole.

Blinds

  • Reed or bamboo blind: reeds or split bamboo twined together with cord every 15–20 cm (Baskets and Containers), rolled up and tied with two cords.
  • Roman blind: cloth with pockets every 20–25 cm holding thin slats, and cords running up through rings sewn on the back; pulling the cords folds it up in pleats.
  • Roller blind: a wooden roller 3–4 cm thick, the width of the window, with the cloth tacked along it. In the simplest kind, a cord wound round one end pulls it up. In the spring roller, the roller is hollow and contains a long coil spring (Springs) fixed at one end to a flat pin that sits in a slotted bracket and cannot turn. Pulling the blind down winds the spring tight. A small pawl (a pivoting catch) drops into a notched ratchet at the end when the blind is still, holding it; a short tug lets the pawl swing free and the spring rolls the blind up. Stiffen the cloth with starch or size (Laundry and Bleaching Cloth) so it rolls flat.

Rugs and carpets

A · FLAT WEAVE (KILIM) bare warp 3–4 per cm weft packed so hard the warp vanishes; a slit opens where two colours meet B · KNOTTED PILE pile ends cut, sheared knot round 2 warps 2–4 weft picks between rows of knots C · RAG RUG cloth strips 2–4 cm wide as weft D · BRAIDED RUG braid 3-strand braid coiled round a centre braid, laced through its loops with strong thread
Fig. 3 Four kinds of rug. Flat weave: a strong warp is completely hidden by weft packed tight. Knotted pile: each symmetric knot wraps two warps and its two ends stand up as pile, with rows of plain weft between. Rag rug: strips of old cloth woven as weft. Braided rug: a three-strand braid of rag strips coiled flat and laced together.

All woven rugs need a strong, tight warp — hard-spun linen, hemp, cotton or wool, 2- or 3-ply — and a heavy beat. A light frame loom bends; use the floor The Loom or build an upright rug loom: two posts 15 cm thick, a fixed beam across the bottom and an adjustable one across the top, wedged apart to make the warp as tight as a drum.

Flat-weave rug (kilim). A weft-faced plain weave: warp about 3–4 threads per cm, weft of thick wool beaten down so hard that the warp disappears completely. Patterns are made by weaving each colour only across its own area and turning back. Where two colours meet on a vertical line, a slit forms; interlock the wefts round a shared warp to close it. Finish the ends by knotting the warp threads in bundles of 4–6 to stop the weft working loose.

Knotted pile rug.

  1. Warp 3–5 threads per cm. Start and finish with 3–5 cm of flat weave.
  2. Tie a row of knots across the warp. The symmetric (Turkish or Ghiordes) knot: lay a short length of pile yarn across two neighbouring warps, wrap each end round one warp, and bring both ends up together between them. The asymmetric (Persian) knot wraps one warp only and lets finer patterns be tied. Cut each knot off the yarn with 2–3 cm ends standing up. Push the row down firmly.
  3. Weave 2–4 rows of plain weft and beat hard with a heavy comb-shaped beater.
  4. Repeat. Every few rows, shear the pile level with scissors or shears to an even length, usually 1–1.5 cm.
  5. Density: a coarse village rug has about 5–15 knots per cm²; fine city carpets 40 and more. A rug of 1 × 1.5 m at 10 knots per cm² has 150,000 knots. An experienced knotter ties a few thousand a day, so plan a month or more.

Rag rug. The rug that uses up worn-out clothes and bedding.

  1. Cut old cloth into strips 2–4 cm wide (thinner for heavy cloth). Join strips end to end by overlapping them and sewing across diagonally, or by cutting a slit in each end and looping one through the other. Roll them into balls.
  2. Warp strong cotton or linen at about 2–3 threads per cm, often in pairs.
  3. Weave in plain weave with the rag strip as weft, folding it into a rough tube as you lay it in. Beat very hard. Start and end with 3–5 cm of plain yarn weft, and knot the warp ends.
  4. Sizes: a bedside rug 60 × 90 cm; a runner 70 cm wide and as long as the hall.

Braided rug. No loom needed.

  1. Cut cloth strips 4–6 cm wide, fold the raw edges to the middle and fold again, so each strip is a smooth tube about 1.5 cm wide.
  2. Braid three strips together tightly. Join new lengths at different points so the joins are spread out.
  3. Coil the braid flat in a spiral (round rug) or round a straight centre length (oval rug: start with a centre braid as long as the rug's length minus its width).
  4. Lace each round to the last with strong linen thread and a blunt needle, passing through the loops of the braids, never through the cloth. On the curves, skip a loop on the outer braid now and then so the rug lies flat; if it cups up, you are lacing too tight; if it ripples, too loose.
  5. Taper the end of the braid and tuck it under.

Carpet. Wall-to-wall carpet is pile or flat weave made in strips about 70 cm wide, sewn edge to edge on the back, laid over an underlay of felt, old blankets or paper, and tacked at the edges (Nails, Rivets and Wire Fasteners). On power looms the pile is formed over wires; a blade on the end of each wire cuts the loops as it is withdrawn (Textile Machinery).

Mats and doormats

  • Rush and reed mats: plaited or twined (Baskets and Containers); the oldest floor covering, and still the cheapest.
  • Rope mat: coil an old rope (8–15 mm) flat in a spiral or an oval, and sew each round to the last with twine through the strands (Ropewalks and Sailcloth). Or plait a flat sennit of three or more strands and coil that.
  • Doormat: about 45 × 75 cm and 1.5–3 cm thick, with stiff, upright fibres that scrape mud off boots. The classic is coir — the coarse fibre of coconut husks (Cordage and Rope) — tied into a pile on a backing, or woven very tightly. A thrummed mat of short rope yarns pushed through stout canvas, as sailors made, does the same. Put a boot scraper — an iron bar set edge-up in a stone or frame — outside the door (Blacksmithing).

Cushions

  1. Pad: cut two squares of ticking 2 cm bigger than the finished cushion (usually 40–50 cm), sew round, leaving a gap, turn, fill firmly with feathers, kapok, wool, or chaff, and slip-stitch the gap closed.
  2. Cover: front the same size as the pad plus 1.5 cm seam allowance; back cut in two overlapping halves (each 2/3 the width), hemmed where they overlap so the pad can be pushed in — an envelope back. Or close it with buttons or ties.

A good cushion springs back when you stand up.

Towels

Terry towelling has loops on both faces. On a hand loom:

  1. Two warps. A tight ground warp of strong cotton or linen, and a pile warp of soft, loosely spun cotton, wound on a second beam (or weighted separately) under light tension. Alternate them: one ground thread, one pile thread.
  2. Three-pick terry. Weave two picks of weft but beat each one only to about 5–10 mm short of the finished cloth. On the third pick, beat fully: all three picks slide together up to the cloth, and because the pile warp is slack, it buckles up into loops 3–5 mm high, on the face or the back depending on the shed. Then let out a little more pile warp and repeat.
  3. By hand: or lift every pile thread over a smooth rod 4–5 mm thick, weave the next ground pick, and slide the rod out. Slower, but needs no special beat.
  4. Weave 4–5 cm of plain cloth at each end for the hem, and hem it double.

Sizes: hand towel 50 × 90 cm; bath towel 70 × 140 cm; face cloth 30 × 30 cm. A good towel feels soft, does not shed lint, and a drop of water on it disappears at once instead of sitting on top. New linen and cotton absorb poorly until washed a few times.

Handkerchiefs

A handkerchief is a square of fine linen or cotton, 30–45 cm across, woven at 30 or more threads per cm. Hem it with a rolled hem: moisten the edge, roll 2–3 mm of it tightly between finger and thumb, and slip-stitch it as you go, 4–5 stitches per cm (Sewing, Needles and Thread). Keep several per person. Used ones carry germs: boil them in the wash (Laundry and Bleaching Cloth), and put them straight into a covered pot when used. During epidemics, paper tissues that are burnt after use are safer (Paper, Infectious Diseases).

How to tell it worked

  • Blanket: even glow against the light, springy nap, no thin lines where teasels tore.
  • Sheets, towels, curtains: square corners, straight hems, the grain running true (pull a weft thread and check that the cut edge follows it).
  • Rugs: lie flat without cupping or rippling; the warp is hidden in flat weaves; pile does not pull out when tugged hard; the rug does not slide on the floor.
  • Blinds: a roller blind stops where you leave it and rolls up straight without drifting to one side.

Note Troubleshooting

  • Blanket thin and hairy → raised too hard or too dry. Raise damp cloth in light passes.
  • Rug won't lie flat → uneven warp tension, or braids laced too tight (cups) or too loose (ripples).
  • Terry loops uneven or missing → pile warp too tight, or the two short picks went right up to the cloth. Slacken it; check the gap before the third pick.
  • Roller blind won't hold → the pawl is stuck or the ratchet is worn. Clean and oil it, or add spring tension by rolling it up by hand two turns before fitting.

Dangers

Danger Blind and curtain cords strangle small children. Loops of cord hanging within reach of a cot, bed or chair are a known cause of child deaths. Cut loops into two separate ends, keep all cords wound on a cleat at least 1.5 m above the floor, and never put a cot beside a corded window.

Danger Babies under one year must not sleep with pillows, duvets, cushions or loose blankets, which can cover their face and suffocate them. Lay them on their back on a firm mattress with a fitted sheet and, if needed, a blanket tucked in firmly at chest height.

  • Fire. Brushed cotton and other light, fluffy cloth catches and burns very fast; a spark or a candle can turn a nightdress or curtain into a sheet of flame. Keep curtains and bedding well away from fires, lamps and candles. Wool is slower to catch and is the safest fibre near a hearth; use fire guards (Firefighting).
  • Tripping. Rugs that slide on smooth floors cause falls, especially for old people. Put a rug on a felt underlay or sew strips of rubber (Rubber) or rough sacking under its corners.
  • Moths and mites. Beat rugs and air bedding in the sun; store wool with cedar or lavender (Household Pests, Mops, Dustpans and Cleaning Tools).

What this unlocks

Weaving towels, sheets and blankets for a whole community is one of the first jobs worth mechanising, and these were among the first products of the power The Loom and Textile Machinery. Clean bed linen and towels are essential in hospitals (Nursing the Sick), and rugs and curtains are the beginning of Insulation and Keeping Buildings Warm or Cool for a warm house.

How it was first done

The oldest surviving pile carpet, the Pazyryk carpet, about 2 × 1.8 m with roughly 36 symmetric knots per cm², was found frozen in a Scythian burial mound in the Altai mountains of Siberia by the Soviet archaeologist Sergei Rudenko in 1949; it is about 2,400 years old. Teasels were used to raise wool cloth in Roman times, and water-powered gig mills appear in England by the 1400s. The Hudson's Bay Company sold its wool "point blankets" from about 1780, with short black lines (points) woven into the edge to show the size. The American Erastus Bigelow built power looms for carpets from 1839. Looped terry cloth came from the Ottoman Empire, where it was woven by hand; mechanised terry weaving was developed near Manchester in the 1850s by W. M. Christy & Sons, and terry towels became common household goods soon after.