◆ Rebuild

Part 2 · Earth and Fire

Bricks

How to make sun-dried mud bricks (adobe) and kiln-fired bricks with a simple wooden mould, fire thousands at a time in a clamp, and lay them with mortar into walls and arches.

Difficulty
●●●●●
Time
A day to mould 300–500 bricks; 2–6 weeks to dry; a week to fire and a week to cool
Steps from zero
3 prerequisites →

You need first

Finding and Preparing ClayThe Kiln

This unlocks

Arches, Vaults and DomesChimneys, Stoves and HeatingSewers and WastewaterFirebrick and Refractories
The full path from nothing — 3 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. The Kiln
  4. Bricks

Do them roughly in this order. See it on the tech tree →

Why it matters

A brick is a stone you can make wherever there is clay, in the exact size and shape you want, by the thousand. With bricks you can build houses that keep out cold, heat and rain; chimneys and ovens that do not burn down your home; kilns and furnaces that last for years; cisterns, drains and wells; and arches and vaults that span openings without any timber at all.

There are two kinds:

  • Mud bricks (adobe) are only sun-dried. They cost nothing but labour and need no fuel. They are excellent in dry climates, but soften and wash away if they stay wet.
  • Fired bricks are baked at 900–1,000 °C into true ceramic. They survive rain, frost and fire for centuries. They cost a great deal of fuel.

Bricks lead to better The Kilns, Firebrick and Refractories for metal furnaces, Mortar and Concrete building, and Roads and Bridges.

How it works

Brick-making is Pottery on a large scale, and follows the same rules. A brick shrinks as it dries and again as it fires, so it needs enough temper — sand, straw or dung — to stop it cracking. It must be dried slowly and completely before firing, or steam blows it apart. And it must be fired hot enough (above about 700 °C, ideally 900–1,000 °C) to become permanent ceramic.

Mud bricks are different only in that they are never fired. The clay is the glue that holds sand and straw together. Straw acts like the steel bars in reinforced concrete: it holds the brick together as it shrinks and stops cracks spreading.

What you need

Item Amount Notes
Brick earth About 2 m³ per 1,000 small bricks Clay-rich subsoil; see "The right earth" below
Sand As needed To temper fat clay
Straw, dry grass or dung Several big bundles For adobe; chopped to 5–10 cm
Water Plenty A pond or stream nearby saves enormous labour
Moulds 2–4 Wooden frames (below)
A flat, level drying floor About 30 m² per 1,000 bricks Swept bare earth sprinkled with sand
Covers Mats, thatch or leaves to shelter drying bricks from rain
Fuel for a clamp Roughly 1–1.5 m³ of stacked dry wood per 1,000 bricks Split wood, brushwood, dung cakes
Mortar Mud for adobe; Lime mortar for fired brick
A plumb line and a level 1 each A stone on a string; see Measurement from Scratch

The right earth

Good brick earth is a sandy clay — not as fat and sticky as the best pottery clay.

  • For adobe: roughly 15–30% clay and the rest sand and silt. A ribbon test (see Finding and Preparing Clay) that breaks at 2.5–5 cm is about right. Too much clay and the bricks crack as they dry; too little and they crumble.
  • For fired bricks: a little more clay, about 25–50%. Most ordinary subsoils that ribbon to 3–6 cm work. Mix sand into very fat clay.
  • Avoid earth with lots of stones, roots, lime (it fizzes with vinegar — see Finding and Preparing Clay) or salt (white crusts on drying earth). Lime and salt both spoil fired bricks.

The test brick. Before making thousands, make ten bricks from your mix. Dry them for two weeks. If they crack, add sand or straw. If they crumble at the corners, add clay. Fire a few. Adjust and test again.

Making the mould

A brick mould is a wooden frame with no top and no bottom, so the brick drops out.

26 cm 12.5 7.5 1 MOULDno top, no bottom;inside 10% over size 2 THROWwet, sanded mould;throw the clot hard 3 STRIKEscrape off the surpluswith a wet stick 4 LIFTlift straight up;the brick stays to dry
Fig. 1 A brick mould and how it is used. The frame has no top or bottom. Throw a clot of clay hard into the wetted, sanded mould, strike off the surplus, then lift the mould straight up and leave the brick to dry.
  • Size. A good all-round fired brick is about 24 × 11.5 × 7 cm when finished — small enough to lift in one hand. Its length is twice its width plus one mortar joint, so bricks can be laid in any pattern. Clay shrinks 5–10% from wet to fired, so make the mould's inside about 10% larger: 26 × 12.5 × 7.5 cm.
  • Adobe blocks are usually larger: about 40 × 20 × 10 cm (weighing 12–15 kg).
  • Build it from four boards about 2 cm thick of smooth hardwood, joined at the corners so it cannot spread. Handles on the ends make it easier to lift. A double or triple mould (two or three bricks side by side in one frame) doubles your output.
  • A strike — a straight flat stick — scrapes surplus clay off the top.

Method 1: Mud bricks (adobe)

  1. Mix. Dig a shallow pit, fill it with earth, and soak it overnight. Add chopped straw or dung — about one part straw to four or five parts earth by volume. Tread it with bare feet (or have animals tread it) until it is even, with no dry lumps. It should be stiff like thick porridge: it holds its shape, but a stick pushed in comes out clean.
  2. Leave it a day if you can. The straw softens and the mix becomes more workable.
  3. Mould. Set the mould on the drying floor and wet its inside. Pack it full of mix by hand, pressing hard into the corners. Strike off the top with the stick.
  4. Lift the mould straight up with a gentle wiggle. Set it down a finger's width from the last brick and repeat. A team of two can make 300–500 adobe bricks a day.
  5. Dry. Leave the bricks flat for 2–3 days, until you can pick them up without denting them. Then stand them on edge to dry on all sides. After about a week, stack them loosely in open rows with gaps between. Full drying takes 2–4 weeks in a dry season.
  6. Protect from rain. Cover them with mats or thatch whenever rain threatens. A rain shower on fresh adobe ruins it.

Method 2: Fired bricks

Moulding

  1. Prepare the clay. Soak brick earth overnight, add sand if it is fat, and tread or wedge it until smooth and even (see Finding and Preparing Clay). Pick out stones. It should be stiffer than adobe mix — like stiff dough.
  2. Sand or water the mould. Either dip the mould in water (slop moulding: bricks come out smoother), or wet it and sprinkle sand inside (sand moulding: bricks release more easily and keep sharper edges).
  3. Throw the clot. Roll a lump a little bigger than the mould in sand, raise it above your head and throw it hard into the mould on a sanded board or the floor. This fills the corners and drives out air. Press the corners with your fingers.
  4. Strike off the surplus with a wet stick. Turn the mould onto the drying floor and lift it off (or lift it straight up if moulding on the floor).
  5. Mark them. A thumb-print or a pressed sign on each brick is useful — and is how archaeologists know who made ancient bricks.

Drying

Exactly as for adobe: flat for 2–3 days, then on edge, then stacked in open "hacks" (loose stacks with gaps) under a cover — for 2–6 weeks depending on weather. Every brick must be bone dry before firing: pale, evenly coloured, and not cool against your cheek. Wet bricks in a clamp explode, and can bring the whole stack down.

Firing in a clamp

A clamp is a kiln made of the bricks themselves. You stack the raw bricks into a big block with fire tunnels underneath, case the outside with mud, and burn fuel in the tunnels. It needs no permanent structure and can fire thousands of bricks at once. (For a few hundred, you can fire them in your The Kiln instead.)

Top glows orange when doneand the whole clamp settles 5–10 cm Casingold fired bricks,plastered with mud Basefired bricks or stone Raw brickson edge, coursescrossing, 1–2 cmgaps between Fire tunnels30 cm wide, 40–50 cm high, about 1 m apart; fed from both ends
Fig. 2 A brick clamp in cross-section. Raw bricks are stacked with finger-wide gaps over arched fire tunnels. Old fired bricks and mud plaster case the outside. Fuel burns in the tunnels for several days.
  1. Base. Choose level, dry ground. Lay a floor of already-fired bricks or flat stones, a little bigger than your clamp. For a first clamp of 3,000–5,000 bricks, plan a block about 3 m long, 2.5 m wide and 2 m high.
  2. Fire tunnels. Across the clamp, build tunnels about 30 cm wide and 40–50 cm high, about 1 m apart, running from one side to the other. Make their walls of raw bricks and corbel the top (step each course in a little until they meet) or span them with long bricks.
  3. Stack the bricks. Above the tunnels, set the raw bricks on edge, with finger-wide gaps (1–2 cm) between them so hot gas can rise through. Lay each course crosswise to the one below, so the stack ties together. Put the biggest, strongest bricks low down.
  4. Case it. Build the outer skin from two layers of old fired bricks if you have them, or the worst raw bricks, and plaster the whole outside with 5 cm of mud mixed with straw. Leave the tunnel mouths open. Cover the top with a layer of bricks laid flat, then a thin layer of earth, leaving a few gaps for the smoke.
  5. Water-smoke (1–2 days). Light small fires at the tunnel mouths. Keep them low. Steam pours from the top. Hold a cold stone over the top: when it no longer fogs, the bricks are dry.
  6. Full fire (2–4 days). Push fuel deep into the tunnels and fire hard, day and night. Feed from both ends if you can. Watch the top: as the heat rises through the stack, the top bricks begin to glow red, then orange at night. The whole clamp settles 5–10 cm as the bricks shrink — a good sign.
  7. Close and cool (5–7 days). When the top glows orange all over and the clamp has settled, stop feeding, brick up and mud-seal the tunnel mouths, and close the top. Let it cool for at least five days. Then take it apart from the top down.

A clamp is uneven. Expect bricks near the tunnels to be overfired — dark, glassy, sometimes warped (good for foundations and paths) — and bricks at the outside edges and top to be underfired — pale and soft (put them in the casing of the next clamp, or refire them). The good, evenly fired middle is usually 60–80% of the load.

How to tell it worked

  • Ring. Knock two bricks together. A well-fired brick gives a clear ring; an underfired one gives a dull thud.
  • Colour. Even red, orange or buff all through when broken. A pale, chalky look means underfired. A black core means the inside did not burn clean — fire longer and more slowly next time.
  • Hardness. A fingernail cannot scratch it; a steel blade only just marks it.
  • Soak test. Weigh a dry brick (on a balance against stones), soak it in water for a day, and weigh it again. A good brick gains less than about 20% of its weight. Underfired bricks soak up more, and soften.
  • Drop test (adobe). A dry adobe brick dropped flat from waist height onto hard ground should only chip at the corners, not break in two.

Note Troubleshooting. Bricks crack in drying → too much clay or dried too fast; add sand or straw, shade them. Bricks burst in the clamp → not dry; water-smoke longer. White crust appears on bricks after rain → salts in the clay or water; wash earth with clean water or dig elsewhere. Small craters pop out weeks later → lime grains in the clay (see Finding and Preparing Clay). Adobe crumbles at the corners → not enough clay; add clay or more straw.

Laying bricks

Foundations

All walls start below ground. Dig a trench down to firm subsoil, at least 50 cm deep (deeper where the ground freezes), and twice as wide as the wall. Fill it with large stones bedded in mortar. Bring this stone footing up at least 30 cm above ground before any adobe goes on: water splashing off the ground is what destroys mud walls.

Mortar

  • Adobe: use mud mortar made from the same earth as the bricks, without straw, sieved.
  • Fired bricks: use Lime mortar — 1 part lime putty to 3 parts sharp sand. Clay mortar works for dry, sheltered walls and inside kilns.

Laying

STRETCHER BONDeach course shifted half a brick;for walls one brick thick ENGLISH BONDstretchers and headers in turn;ties a two-brick wall together ARCH ON A CENTRING Keystone Centringtemporarywooden former pushpush Wedges and propsknock out after a week Abutmentsheavy enough to resist
Fig. 3 Brick bonds and a simple arch. In every bond, each vertical joint sits over the middle of the brick below. An arch is built on a temporary wooden centring and finished with the central keystone; the walls beside it must be strong enough to resist its sideways push.
  1. Wet fired bricks before laying (dip them in water), so they do not suck the water out of the mortar. Do not wet adobe.
  2. Corners first. Build up each corner a few courses, checking it is upright with a plumb line and level with a water level or a straight board and a plumb bob (see Measurement from Scratch).
  3. String line. Stretch a cord between the corners at the top of the next course, and lay each brick to the line.
  4. Bed and joint. Spread a bed of mortar about 1 cm thick, butter one end of the brick, press it down and slide it against its neighbour. Tap it level. Scrape off squeezed-out mortar. Joints should be full — gaps let in water.
  5. Break the joints. Each vertical joint must sit over the middle of a brick below. Never let vertical joints line up from one course to the next; that makes a crack waiting to happen.
    • Stretcher bond: all bricks laid lengthwise, each course shifted half a brick. For walls one brick thick.
    • English bond: courses of bricks laid lengthwise (stretchers) alternate with courses laid crosswise (headers), tying a wall two bricks thick together.
  6. Do not build too fast with lime mortar. About 1–1.5 m of height per day, so the lower courses can stiffen.

Wall thickness. For a single-storey house, fired brick walls should be at least one brick length thick (about 24 cm), and adobe walls 30–45 cm. Keep a wall's height less than about 10 times its thickness unless it is braced by cross-walls.

Arches

An arch carries weight around an opening by pressing each brick against its neighbours. It needs no wood once finished — but it needs support while being built.

  1. Make a centring: a wooden former shaped like the inside of the arch — for a doorway, a half-circle cut from planks, or a frame of bent saplings covered with boards. Prop it in place on wedges.
  2. Lay from both sides at once. Start at the springing points (where the arch begins) and work up both sides evenly, setting bricks on end around the curve. Use thin mortar joints at the inside and thicker at the outside — or shape bricks into wedges before firing.
  3. Key it. The last brick at the top — the keystone — is pushed in tight, locking the arch.
  4. Wait. Leave the centring in place until the mortar has set: at least a week for lime mortar, longer for big arches. Then knock out the wedges so the centring drops gently. Stand clear.
  5. Resist the push. An arch pushes outward on its sides. The wall on each side (the abutment) must be thick and heavy enough not to be pushed over — at least as wide as a quarter of the span for a small arch, more for a flatter one. A semicircular arch pushes least.

Tip Vaults without wood. In Egypt and Nubia, builders have long roofed rooms with mud brick and no centring at all: they lean each ring of bricks against the one before, starting from a solid end wall, so every ring is supported while the mortar sets. This "Nubian vault" needs practice but no timber.

Dangers

Danger Collapsing walls and arches kill. An unbonded, too-thin or too-tall wall can fall without warning, and so can an arch whose centring is removed too early. In earthquake country, unreinforced brick and adobe buildings are the most dangerous places to be (see Building Against Earthquakes and Storms). Bond every course, keep walls thick and braced with cross-walls, tie the top of the walls together with a continuous timber beam, and never stand under fresh arches.

  • Clamp fires burn for days, throw sparks and give off carbon monoxide; keep the clamp well away from houses and stores, and do not sleep near it.
  • Collapsing clamp. A clamp can slump or burst while burning, especially if bricks were wet. Keep people away from its sides during the full fire.
  • Heavy work. A fired brick weighs about 3 kg; a thousand weigh three tonnes. Lift with your legs, share the work, and pass bricks hand to hand rather than carrying great loads.
  • Lime mortar burns skin and eyes — see Lime.
  • Clay pits fill with water and have steep, slippery sides. Fence them; children drown in them.

Going further

How it was first done

The earliest known bricks are hand-shaped mud bricks from Jericho, in the Jordan Valley, made around 9000–8000 BC; some still carry the builders' thumbprints. Bricks made in wooden moulds appeared in Mesopotamia a few thousand years later. Fired bricks became common there and in the Indus Valley by about 3000 BC; the planned cities of Harappa and Mohenjo-daro (around 2500 BC) used millions of standard-sized fired bricks. The Romans spread fired brick and the arch across Europe. Adobe is still one of the most common building materials in the world, and many millions of people live in earth-built homes today.

Source: content/entries/earth/bricks.md