The saddler's and harness-maker's trade. It covers making the tools (round knife, swivel knife, stamps, edge tools and the stitching horse), choosing and cutting a hide, stitching to carry heavy loads, tooling and carving patterns, dyeing and finishing, and moulding wet leather. It then shows how to make the bridle, harness and riding saddle, plus straps and moulded cases.

Difficulty
●●●●●
Time
An afternoon to make a swivel knife; two days for a stitching horse; a week for a bridle; a month or more for a full cart harness or a riding saddle
Steps from zero
6 prerequisites →

You need first

Hides and LeatherSewing, Needles and Thread

This unlocks

Bits, Stirrups and Spurs
The full path from nothing — 6 steps before this one
  1. Cordage and Rope
  2. Stone Tools
  3. Hunting and Trapping
  4. Spinning and Weaving Cloth
  5. Hides and Leather
  6. Sewing, Needles and Thread
  7. Leatherwork and Harness-Making

Do them roughly in this order. See it on the tech tree →

Why it matters

Hides and Leather tells you how to tan a hide, and Bags, Backpacks, Wallets and Luggage teaches the basic skills: cutting, the saddle stitch, skiving, burnishing, wet moulding and fitting rivets and buckles. This chapter is the next step up, the trade of the saddler and harness-maker. Their work has to carry hundreds of kilograms of pull, day after day, in rain and sweat, on a living animal that is hurt by any badly placed edge. A horse or ox in good harness ploughs, hauls and carries for twenty years (Draft Animals and Harness, Wagons and Carriages). A bad harness galls the animal and breaks at the worst moment.

The same skills make belts, machine belting, pump and bellows leathers, and cases for instruments and tools.

How it works

  • Only vegetable-tanned leather tools and moulds. Bark tannin leaves the fibres able to be compressed and set when damp. Brain-tanned or oil-tanned leather springs back and won't hold a line.
  • Casing. Damp leather takes an impression; dry leather resists it; soaking-wet leather mushes. The right state is called cased: wet through, then left until the surface is back to almost its dry colour. Press the leather to your cheek: it should feel cool but not wet.
  • Which part of the hide. The firm, even leather along the spine and over the rump (the bend) stretches least, so cut it into traces, reins, girth straps and anything that takes pull. The shoulder is slightly softer, good for tooling and saddle skirts. The belly stretches and is thin and loose; use it for linings, keepers and padding, never for load straps. Cut straps along the backbone, not across it, because leather stretches more across the body.
  • Strength. A sound strap of bark-tanned bend 25 mm wide and 4 mm thick holds very roughly 200 kg in a steady pull. Every hole, cut and stitch line weakens it, and leather loses strength wet. Harness-makers double the leather (two layers stitched together) on anything that pulls, and aim to make every strap five times stronger than the load.

What you need

Tool Use Make it from
Round knife (head knife) Long straight and curved cuts, skiving Steel (Axes, Chisels, Knives and Planes)
Draw gauge or strap cutter Cutting straps to width Wood and a blade
Swivel knife Carving lines for tooling Steel blade, brass or wood barrel
Stamps Bevelling, backgrounding, patterns Iron rod or hardwood
Edge beveller, edge creaser Rounding and finishing edges Steel
Pricking iron or wheel Marking even stitch spacing Steel
Awl, two needles Stitching Needles and Pins
Stitching horse Holding work Hardwood
Maul or mallet Striking stamps and punches Hardwood, rawhide or horn
Marble or stone slab Hard surface for tooling Smooth slate or marble, 3+ cm thick
Thread Stitching Linen or hemp, waxed (Flax, Hemp and Linen)

Where to find it

Leather comes from Hides and Leather: for harness and saddles you want bark-tanned cattle hide, 3.5–5 mm thick, well curried (worked with fat). Stain and dye ingredients: oak galls and bark (tan), walnut hulls (brown), and scrap iron in vinegar for black (Dyes and Mordants, Vinegar and Pickling). Neatsfoot oil is the oil rendered by boiling the shin bones and feet of cattle; skim it, and let it stand in the cold so the hard fat settles out. It is the classic harness oil because it stays soft and does not go rancid quickly. Beeswax (Beekeeping) and tallow make finishing and thread wax. Ash and beech make trees and frames; boxwood, bone and antler make burnishers and creasers.

Making the tools

Round knife 12–15 cm blade, bevel on top only Yoke forefinger here; does not turn Barrel 10–12 mm, spins Blade 6–10 mm, angled, mirror-stropped Swivel knife maul, not hammer Beveller stamp face slanted, finely ridged Edge beveller notched tip Creaser bone or warm steel, grooved TOOLED LEATHER, CUT THROUGH Swivel cut Bevel Background Next cut Cut half-way through cased leather, then press the outer side down: the raised parts are the design.
Fig. 1 The leatherworker's cutting and tooling tools. The round knife cuts and skives. The swivel knife turns in the fingers to carve smooth curves. Its yoke takes the forefinger and the barrel spins freely. The bevelling stamp presses one side of the cut down, and the edge tools round and crease edges.

The round knife

A half-moon blade 12–15 cm across, on a short wooden handle in the middle of its back. Forge it from good steel, harden and temper it to a light straw colour (Blacksmithing, Steel). Grind a bevel on the top face only, about 20°, leaving the underside flat, and polish it to a mirror on a fine stone and leather strop (Sharpening and Honing). Push the knife away from you, rocking it, for curves; tilt it for skiving. A good one shaves hair off the arm and slices 4 mm leather in one stroke without dragging.

The swivel knife

The swivel knife cuts shallow lines (about half the thickness of the leather) into cased leather. These are the outlines of a tooled or carved design. You pull it towards you while turning the barrel with your fingertips, so it cuts curves as smoothly as a pencil draws them.

  1. Barrel. Turn a brass or hardwood cylinder 10–12 mm across and 8–9 cm long, with knurled or grooved sides for grip (The Lathe, Wood Turning and Treen).
  2. Yoke. On top fit a U-shaped saddle about 2.5 cm wide on a pin running down the barrel's centre, so the barrel spins freely under it. A brass washer and a drop of oil help. The yoke must not turn with the barrel.
  3. Blade. Make a flat steel blade 6–10 mm wide, 1.5–2 mm thick, set into a slot in the bottom of the barrel and held with a screw. Grind the edge straight but angled about 15° to the barrel's base, so that it cuts with its front corner tip down. Grind both faces to a slim double bevel, about as fine as a chisel, and strop it to a mirror. A swivel knife that is not mirror-polished tears the grain instead of cutting it.
  4. Use. Put your forefinger in the yoke, thumb and middle finger on the barrel, and tilt the knife slightly forward so only the corner cuts. Pull it towards you with steady pressure, turning the barrel to steer. Lift at the end of each line, never in the middle of a curve.

A good swivel knife leaves a clean, even-depth line with no ragged edges. Strop it every few minutes of work.

Stamps

Stamps are short iron rods 10–12 cm long with a shaped face that is pressed or struck into cased leather. File the face to shape and leave it fine-textured, not polished, so it burnishes the leather dark (Files and Saws).

  • Beveller: a face 6–8 mm wide, slanted on one side and finely ridged. Walked along one side of a swivel cut, it presses that side down so the design stands up in relief.
  • Backgrounder (tiny dots or grid) beats the background flat and dark; pear shader (a teardrop) hollows leaves and petals; seeders and border stamps repeat small shapes into patterns.

Strike with a hardwood or rawhide maul, never an iron hammer, which ruins the stamp heads.

Edge tools

  • Edge beveller: a short steel blade with a small U-shaped or V-shaped cutting notch at its tip, pushed along the corner of a cut edge to take off a thin curl. Make it from a strip of steel 3 mm thick and file the notch with a small round file. Choose a notch width to suit the leather thickness: about 1 mm for thin leather, 1.5–2 mm for harness.
  • Edge creaser: a steel or bone blade with a groove or a single fence, heated (for steel) to the point where a drop of water sizzles gently and then pressed along a damp strap 2–3 mm from the edge. It burnishes a dark line that stops the edge spreading and makes it look finished.
  • Pricking iron: a row of slanted, sharpened teeth set at the stitch spacing, struck lightly to mark (not pierce) the holes. For harness, 8 stitches to 2.5 cm; for fine bridle work 10–12. A pricking wheel (a toothed wheel on a handle) does the same on long straps.

The stitching horse

The stitching clam in Bags, Backpacks, Wallets and Luggage is held between the knees. For long straps and saddle work the trade used a stitching horse: a bench you sit astride, with a pair of jaws that a foot pedal closes. Both hands are then free for the two needles, and you can open and move the work in a second.

Jaws, faced with leather meet along 12–15 cm and grip the work Fixed jaw 6 × 12 cm ash, wedged into the bench Two needles saddle stitch Hinged jaw 35 cm above the seat Pivot pin Link rod through a slot Foot pedal press to close; lift to open Seat about 50 cm high, sit astride bench 100–120 cm
Fig. 2 The stitching horse. The rider sits astride the bench. The fixed jaw is mortised into the bench; the hinged jaw is pulled shut by a strap or rod from the foot pedal and opens when the foot lifts.
  1. Bench. A board of hardwood 100–120 cm long, 25 cm wide and 5 cm thick, on three or four splayed legs, with the seat about 50 cm from the floor (knee height when seated).
  2. Fixed jaw. An upright of ash or beech 6 × 12 cm with its foot let into a slot near the front of the bench and wedged or pegged firm, rising so its top is about 35 cm above the seat, at chest height for close work.
  3. Hinged jaw. A matching upright, hinged at its foot to the bench just in front of the fixed jaw with a stout iron pin, so its top can swing towards and away from the fixed jaw.
  4. Faces. Shape both jaw tops to meet along a line 12–15 cm long. Line the inner faces with leather glued or tacked on, so they grip without marking the work.
  5. Pedal and link. Hinge a foot pedal (a board 30 × 10 cm) under the far end of the bench. Run a strap or iron rod from the pedal, through a hole in the fixed jaw, to the hinged jaw. Pressing the pedal pulls the jaws shut. Add a notched bar or ratchet so the pedal stays down without constant pressure (Cranks, Cams and Linkages). A leaf spring or a loop of rubber cord (Elastic and Rubber Thread) opens the jaws when you lift the pedal.

A good stitching horse grips a strap so hard you cannot pull it out with one hand, opens the moment you lift your foot, and doesn't rock as you stitch. If the work slips, re-face the jaws or lengthen the pedal lever.

Stitching for strength

Harness stitching is the saddle stitch of Bags, Backpacks, Wallets and Luggage made heavier and tighter:

  1. Thread. Twist 6–10 strands of linen or hemp, wax them with a mix of beeswax, pine resin and a little tallow, and taper the ends to fit the needles (Sewing, Needles and Thread).
  2. Mark a groove 4–5 mm from the edge, prick it at 8 stitches to 2.5 cm, and pierce each hole with a diamond-section awl held at the same slant every time.
  3. Stitch both needles through each hole, pulling each stitch down hard, so the thread beds into the groove.
  4. Lock the ends by back-stitching four holes. Never knot them; knots work loose and cut.
  5. Doubling. For traces, reins and girth straps, glue or tack two layers flesh to flesh, stitch both edges, then bevel, sand, crease and burnish the edges as one.

Tooling and carving

  1. Case the leather: wet it through, then leave it in a closed box or damp cloth for an hour or two until the surface is almost dry-coloured.
  2. Transfer the design. Draw it on thin paper, lay the paper on the cased leather, and trace the lines with a blunt stylus so they show faintly.
  3. Cut the main outlines with the swivel knife to about half depth.
  4. Bevel along the outside of each cut, overlapping each blow by half the tool's width, with steady, even mallet strokes, so the outer side sinks and the design rises.
  5. Background, shade and decorate with the stamps. Finish with fine decorative cuts made with the swivel knife (thin, tapering lines on leaves and scrolls).
  6. Dry slowly, away from the fire, before dyeing.

If the leather dries as you work, dampen it from the back with a sponge.

Dyeing and finishing

  • Iron black (often called vinegaroon): put a handful of clean rusty iron scraps or nails in a litre of vinegar for a week or two, until it stops fizzing and turns dark grey. Brush it on bark-tanned leather; the iron reacts with the tannin and turns it jet black in seconds. For leather that is pale or has little tannin, paint on oak-gall or strong bark tea first. Rinse and oil afterwards, because the acid dries the leather.
  • Browns from boiled walnut hulls, onion skins or strong bark liquor, brushed on in thin coats (Dyes and Mordants).
  • Oil a newly dyed, dry piece with a thin coat of warm neatsfoot oil on the flesh side and the grain. It darkens the leather a little and keeps it supple. Too much oil makes it soft and floppy and draws dirt.
  • Wax the surface with beeswax and tallow, buff it with a cloth, and burnish the edges.
  • Care. Wipe wet harness clean, dry it slowly away from the fire, and oil it lightly every few weeks of hard use.

Wet moulding and cases

Moulding is described in Bags, Backpacks, Wallets and Luggage. For a leather case, such as for spectacles, a knife, a surveyor's instrument or a bottle, carve a wooden form 1–2 mm larger than the object all round. Stretch cased leather 2–3 mm thick tightly over it, pressing it into every corner with a bone tool. Tack it to the base, and let it dry for two days. Then cut it free, stitch any seam with a welt (a narrow strip of leather between the edges), and finish the rim. A lid is made the same way over a form slightly larger again. For a stiff, hard case, dip the moulded leather in water at 60–80 °C for a minute before the final shaping (cuir bouilli).

Harness

The collar, hames, traces and whippletree, and how they carry the pull, are in Draft Animals and Harness. Here are the leather parts and how to make them. Measure each animal with a cord or tape, and make every strap with at least three holes for adjustment each way from where it will normally buckle.

Blinker Bit and noseband Browband Headpiece and throatlatch Collar and hames see Draft Animals Cart saddle arches clear of the spine Shaft tug and belly band carry and hold down the shafts Loin strap holds up the breeching Crupper Breeching 8–10 cm, doubled Traces and shaft reins to driver
Fig. 3 The leather parts of a cart-horse harness and the bridle. The bridle carries the bit; the cart saddle and belly band carry the shafts; the breeching lets the horse hold the load back.

The bridle

  • Headpiece passes behind the ears and splits into the cheekpieces, which run down the face to the bit rings (Bits, Stirrups and Spurs), and the throatlatch, which buckles loosely under the throat. You should be able to fit a fist under the throatlatch.
  • Browband across the forehead, about 38–42 cm for a cart horse, keeps the headpiece from slipping back.
  • Noseband about 5 cm below the cheekbones; two fingers should fit under it.
  • Blinkers (stiff leather cups on the cheekpieces) for driving horses.
  • Cheekpieces are set so the bit makes one or two small wrinkles at the corners of the mouth.
  • Width: 16–22 mm for riding bridles, 22–25 mm for working bridles. Use single-thickness bend leather 3.5–4 mm, stitched at every fold; buckles of forged iron or cast brass (Buttons, Buckles, Hooks and Zips).

Reins: for riding, about 2.7 m in all — two halves of about 1.35 m each, buckled together at the hand — 16–22 mm wide, buckled or stitched to the bit. For driving from a cart, 5.5–6 m each side, 22–25 mm wide, the hand part sometimes widened or plaited for grip.

Cart saddle, belly band and breeching

  1. Cart saddle (back pad): a padded leather pad on a narrow wooden or iron tree that arches clear of the spine. It carries the back band and the shaft tugs (loops for the cart shafts). Stuff its panels with wool or straw as for a collar.
  2. Belly band under the girth area holds the shafts down, so a light load cannot tip them up.
  3. Crupper: a padded loop under the root of the tail, joined to the saddle by a back strap. It stops the cart saddle sliding forward. Stuff the dock piece round and smooth, about 3 cm thick, and keep it clean; dirt here causes sores quickly.
  4. Breeching: a broad strap 8–10 cm wide, double thickness, passing round the hindquarters about 25–30 cm below the root of the tail, held up by straps over the loins. Short side straps buckle it to the shafts. A hand's width should fit between it and the buttocks when the horse stands square. Too loose and the cart runs onto the horse going downhill; too tight and it chafes on every step.

A harness fits when, under load, every strap lies flat and straight, no buckle or stitch line touches a bony point, and after a day's work the sweat marks are even with no dry patches or rubbed hair.

The riding saddle

A riding saddle spreads the rider's weight over the long muscles on either side of the horse's spine, as the pack saddle does in Pack Animals, while keeping the rider balanced in the right place (Riding and Training Horses).

SIDE VIEW, PULLED APART FROM THE FRONT Seat cover one cased piece Ground seat layers, skived Cantle Front arch stirrup bar, opens to the rear Tree bars 45–55 cm, rawhide-covered Panels stuffed with wool Girth 110–135 cm, two buckles each side Stirrup 2 cm wider than boot 5–8 cm over the withers gullet 6–8 cm wide, clear the full length Bars rest on muscle Front arch (fork)
Fig. 4 A riding saddle pulled apart. A wooden tree of two bars, a front arch and a cantle, covered in shrunk rawhide, carries everything. The seat is built up in layers of leather. Stuffed panels sit under the bars, and the girth and stirrup leathers buckle to the tree.

The tree

  1. Bars. Shape two boards of ash, beech or poplar 45–55 cm long, 9–11 cm wide and about 2 cm thick, twisted along their length to lie flat on the horse's back. Carve them using a plaster or clay cast of the horse's back as a guide (Gypsum and Plaster of Paris).
  2. Front arch (fork): a strong arch of naturally curved hardwood, or two pieces joined, fixed across the front of the bars with glue and pegs. Its underside must clear the withers by 5–8 cm (three or four fingers) with a rider seated.
  3. Cantle: a lower arch across the back, shaped to the rider's seat.
  4. Gullet. The gap between the bars is a channel 6–8 cm wide that runs the full length. Nothing must touch the spine.
  5. Rawhide cover. Soak green rawhide (Hides and Leather) until limp, stretch it over the whole tree, lace it tight with rawhide thongs, and let it dry. It shrinks as hard as horn and binds every joint. This is how most strong working trees were made.
  6. Stirrup bars: forged iron hooks bolted to the bars just behind the front arch, open at the rear so a stirrup leather will pull free if the rider falls and is dragged.

Seat, skirts and panels

  1. Ground seat: build up the seat on the tree in layers of firm leather, each a little smaller than the one below, skived to blend. The deepest point should sit in the middle third of the saddle, so the rider sits balanced over the horse's centre.
  2. Seat cover: one piece of well-cased leather stretched over the ground seat, tacked under the arches, and stitched to the skirts.
  3. Skirts and flaps of 4 mm shoulder leather hang down the sides and protect the rider's legs. Tool them now if wanted.
  4. Panels under the bars: leather or wool-cloth bags stuffed firmly and evenly with wool, laced to the tree. They must touch the horse evenly from front to back. Refill them as the wool packs down.

Girth and stirrups

  • Girth: a band 8–10 cm wide of doubled leather, woven webbing (Tablet and Band Weaving) or a row of cords, about 110–135 cm long for a horse, buckled to two straps (billets) on each side, which are fixed to the tree. Always use two buckles each side; one can fail.
  • Stirrup leathers: 2.5–3 cm wide, 1.3–1.5 m long, bend leather, with holes every 2.5 cm.
  • Stirrup irons: forged iron (Bits, Stirrups and Spurs), with a tread about 2 cm wider than the rider's boot. Too narrow traps the foot; too wide lets it slip right through.

Fitting. With the saddle on, ungirthed: it sits level, the front arch clears the withers by three fingers, the gullet clears the spine all the way, and the bars bear evenly with no rocking or gap in the middle. After a ride, look at the sweat mark. Even dampness is right. Dry patches mean pressure points that cut off sweat glands; adjust the panel stuffing there.

How to tell it worked

  • Straps pulled hard over a corner show no cracking on the grain.
  • Stitches lie in a straight, even groove, all equally tight, with no thread fraying on the surface.
  • Edges are round, smooth, dark and glassy, and creased evenly.
  • Tooled lines are crisp; bevels are even with no "stair-steps" between blows.
  • The animal works without rubbed hair, swellings or sore spots after several days.

Note Troubleshooting.

  • Swivel cuts ragged → the blade is dull or the leather too dry. Strop and re-case.
  • Tooling fades → the leather was too wet. Let it dry back to near its own colour.
  • Iron black comes out grey or patchy → the leather was low in tannin or oily. Wash with a weak soda solution, apply bark tea, then re-apply.
  • Straps stretching in use → cut across the hide or from the belly. Recut from the bend.
  • Saddle rocks front to back → the bars curve more than the horse's back ("bridging" is the opposite: a gap in the middle). Re-stuff the panels to match, or reshape the bars.

Dangers

Danger Harness failure kills. A breaking trace, rein or breeching on a hill can run a loaded cart over horse and driver. Inspect every strap, stitch and buckle before each day's work. Replace any strap that is cracked, worn thin at a buckle, or rotted, and never mend load-bearing straps with knots or wire.

  • Knives. Round and swivel knives are razor-sharp. Cut away from your body and hands, on a firm surface, and keep the off hand behind the blade.
  • Stirrups and falls. A foot trapped in a stirrup can drag a fallen rider to death. Use stirrup bars that open to the rear, irons of the right width, and boots with heels.
  • Saddle sores and galls become infected and can disable an animal for months (Animal Health).
  • Iron black and dyes sting eyes and cuts. Wear gloves. Make vinegaroon in a jar with a loose lid, because it gives off hydrogen gas while the iron dissolves; keep it away from flame.

What this unlocks

Good harness lets animals pull ploughs, wagons and mills (The Plough, Animal Power and Treadwheels). Leather belting drives machinery (Belts, Chains and Power Transmission), and cup leathers seal pumps and hydraulic rams (Hydraulic Presses and Rams, Packing, Gaskets and Seals). The The Sewing Machine later takes over long straight seams, but heavy harness and saddles are still largely sewn by hand.

How it was first done

People have cut and stitched leather for tens of thousands of years; bone awls are among the oldest tools found. Egyptian leatherworkers of 3,000 years ago used half-moon knives almost the same as the modern round knife. The Scythians of the steppe rode on padded saddles by about 500 BC, and frozen tombs at Pazyryk in the Altai mountains have preserved felt and leather saddles and harness with rich decoration. Roman cavalry rode on a four-horned saddle that probably had a wooden tree, and stirrups appeared in China around the 4th century AD and spread west over the following centuries. Medieval European saddlers and harness-makers formed guilds and fixed standards for their work. Floral carving with the swivel knife grew up among Mexican and Californian saddle makers in the 1800s and became the well-known "Western" style of tooled leather.

Source: content/entries/textiles/leathercraft.md