Zinc boils away before its ore will smelt, so it cannot be made in an open furnace. Trap its vapour in hot copper to make brass, or distil it in sealed clay retorts as Indian and Chinese smelters did — then use brass for instruments and fittings, and zinc for batteries and rust-proof iron.

Difficulty
●●●●●
Time
A day to roast ore; 8–12 hours per cementation melt; a week to build and dry a retort furnace, then a day per run
Steps from zero
12 prerequisites →

You need first

Copper SmeltingFinding and Identifying Ores

This unlocks

Dry Cells and Electric TorchesGermanium, Gallium and Compound SemiconductorsHorns, Pianos, Organs and Accordions
The full path from nothing — 12 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Bellows
  12. Copper Smelting
  13. Zinc and Brass

Do them roughly in this order. See it on the tech tree →

Why it matters

Brass — copper with a fifth to two-fifths zinc — is golden, does not rust, casts beautifully, machines cleanly, can be drawn into fine wire and pressed into thin sheet, and is not magnetic. It became the metal of precision: clock wheels (The Mechanical Clock), compass cases (The Compass), scientific instruments, screws, pins, hinges, taps, valves and pipe fittings (Pipes, Plumbing and Aqueducts), and horns and bells (Musical Instruments). Brass with half zinc melts low enough to be a brazing filler that joins iron and copper strongly (see Soldering and Brazing).

Zinc on its own is the fuel of electricity: the negative plate of nearly every early The Battery and the can of the dry cell. A coat of zinc on iron — galvanising — stops it rusting even where the coat is scratched. Zinc dissolved in acid makes a soldering flux; zinc oxide is a brilliant white paint (Pigments, Paints and Varnish).

Zinc is also one of the hardest common metals to make, for a reason that surprised metal-workers for two thousand years. This chapter explains why, and gives the two old ways around it.

How it works

Zinc ores are common, and turning zinc oxide into metal with charcoal is ordinary chemistry. The trouble is the temperatures:

0 °C2004006008001,0001,200 no glowdull redcherry redorangeyellow zinc is a liquidzinc is a gas 420 °Czinc melts 907 °Czinc boils about 1,000 °Ccharcoal frees zincfrom its ore 1,085 °Ccopper melts The zinc problem By the time the ore gives up its zinc, the zinc has already boiled. In open air its vapour burns to white smoke.
Fig. 1 Why zinc is difficult. Zinc oxide only gives up its oxygen to charcoal above about 1,000 °C — but zinc boils at 907 °C. So the metal is born as a vapour.
  • Zinc melts at 420 °C and boils at 907 °C (a cherry-red to orange heat).
  • Charcoal only takes the oxygen out of zinc oxide above about 1,000 °C.

So in any furnace hot enough to free zinc, the zinc comes off as a vapour. In an open furnace, that vapour meets air at the top and burns back into white zinc oxide smoke. Old smelters found it as a white fluffy crust on their chimneys ("philosophers' wool") and never saw the metal. There are two ways round this:

  1. Cementation — make brass directly. Hot copper soaks up zinc vapour like a sponge. If copper granules are heated with zinc ore and charcoal in a closed crucible, the zinc vapour goes into the copper before it can escape, and the copper becomes brass. You never see zinc metal. This works only up to about 28–33% zinc.
  2. Distillation — make zinc metal. Heat zinc ore with charcoal in a sealed retort with no air inside, and lead the vapour into a condenser — a tube kept between 420 and 900 °C — where it turns to liquid zinc and drips out. This is harder, but it gives pure zinc for batteries, galvanising and any brass you want.

What you need

Item Amount Notes
Zinc ore — calamine or sphalerite 2–5 kg per run Roasted and powdered; see below
Copper 1–2 kg per cementation Cut into small scraps or thin strips. See Copper Smelting
Charcoal Powdered, plus fuel See Charcoal
Fireclay and grog For crucibles, retorts and condensers See Finding and Preparing Clay and Firebrick and Refractories
Crucibles with lids 2–3, holding 1–3 litres Thick-walled, well fired
Bellows and a crucible furnace See Bellows, Copper Smelting
Retorts and condensers 6–20 For distillation; see Method 2

Where to find it

Zinc ores occur with lead ores, in veins and replacement bodies in limestone country (see Finding and Identifying Ores and Lead). If you find galena, look for zinc beside it.

  • Calamine is the old miner's name for the weathered zinc ores near the surface — mainly smithsonite (zinc carbonate) and hemimorphite (a zinc silicate). Look for crusts, knobbly rounded masses and porous honeycomb lumps ("dry-bone ore") that are white, grey, brown, yellowish, pale blue-green or pink, and heavier than limestone. Smithsonite fizzes in warm vinegar. Calamine is the ore for beginners: it needs no roasting off of sulfur.
  • Sphalerite (zinc blende, "black jack") is zinc sulfide, the main zinc ore deeper down: resinous to glittering, yellow, honey-brown, red-brown to black, breaking into many shiny flat faces. Its streak is pale yellow to light brown — much paler than the mineral. Scratched or crushed and wetted with acid, it may smell of rotten eggs. It is about 4 times heavier than water — clearly lighter than galena.

Tip The charcoal test for zinc. Put a few grains of powdered ore mixed with a pinch of charcoal dust in a hollow on a charcoal block and blow on it hard with a blowpipe, or heat it in the hottest spot of a forge. Zinc ore leaves a coating on the charcoal around it that is yellow while hot and white when cold. No other common metal does that.

Preparing the ore

  1. Pick the ore clean of limestone, galena and quartz. Wash it.
  2. Roast it. Calamine: heat to a dull red (600–800 °C) for 2–3 hours to drive off carbon dioxide and water; it becomes lighter, chalky and crumbly. Sphalerite must be roasted much longer, crushed fine, in a thin layer, stirred often at a dull to cherry red for 6–12 hours, until it no longer smells of burning sulfur — exactly like roasting galena in Lead. Roast outdoors, upwind.
  3. Grind the roasted ore to a powder that passes through a cloth sieve.

Method 1: Cementation brass (calamine brass)

This is how the Romans and medieval Europeans made brass, and the best first step.

Lid sealed with fireclayleave one 5 mm vent Flame at the ventsmall blue-green flame = zinc;white smoke = too hot Charcoal powder2 cm on top Copper pieces2–5 mm thick, in layers Calamine + charcoal2–3 parts roasted calamine,1 part charcoal, per 2 copper Zinc vapoursoaks into the hot copper blast Hold 6–10 hours at cherry red to orange (900–1,000 °C), then yellow to melt.
Fig. 2 Cementation in a closed crucible. Zinc vapour from the ore and charcoal is trapped by the lid and soaks into the copper pieces.
  1. Prepare the copper. Cut copper into small pieces, thin strips or coarse filings — the more surface, the faster it takes up zinc. Pieces 2–5 mm thick are good.
  2. Mix the charge. By weight: 2 parts copper, 2–3 parts roasted calamine powder, 1 part charcoal powder. Moisten the calamine and charcoal slightly so they pack. For a first try: 600 g copper, 800 g calamine, 300 g charcoal.
  3. Pack the crucible in layers: calamine-charcoal mix, then copper pieces, then mix, then copper, ending with a thick layer of mix and then 2 cm of pure charcoal powder on top.
  4. Close it. Put on the lid and seal it with fireclay, leaving one small hole (about 5 mm) so gases can escape without bursting the crucible. Let the seal dry.
  5. Heat slowly in a charcoal furnace. Over an hour, bring it to a bright cherry-red to orange (about 900–1,000 °C) — hot, but not yet hot enough to melt copper. Hold it there for 6–10 hours, feeding charcoal round the crucible.
  6. Watch the vent. A small blue-green to white flame at the hole is zinc vapour burning — a good sign. Billows of white smoke mean too much zinc is escaping: the fire is too hot for this stage. Cool it a little.
  7. Melt. When the vent flame dies down, raise the fire to a full yellow (1,000–1,100 °C) for 20–30 minutes. The copper, now brass, melts at a lower heat than copper did, and runs together at the bottom.
  8. Pour or cool. Break off the lid, skim, and pour into an ingot mould, or let it cool in the crucible and break it out.

Expected result: the ingot should weigh 20–40% more than the copper you put in, and be golden yellow instead of pink. That extra weight is the zinc. If it weighs less than about 15% more, try finer copper, more calamine, and a longer time at the lower heat.

Method 2: Distilling zinc metal

To get zinc metal, you must heat the ore with charcoal in a closed vessel and condense the vapour out of contact with air. The most elegant way is the downward distillation used at Zawar in India: the retorts stand upside down, with their condensers pointing down through the floor of the furnace into a cooler chamber below.

Upper chamberfuel packed roundthe retorts; yellow,1,100–1,200 °C blast Clay plate5–8 cm, pierced Lower chambercooler: dull redat most Retort, mouth downroasted ore + half itsweight of charcoal Clay sealno air may get in Condenservapour turns to liquid zinc Openingslet heat out Cups catch the zinc
Fig. 3 A downward-distillation zinc furnace. Retorts stand mouth-down in the hot upper chamber; zinc vapour passes down the condenser tubes, through the perforated floor, into the cooler chamber, and drips into pots as liquid zinc.

Retorts and condensers

  1. Mix fireclay with an equal volume of grog and a little chopped straw (see Firebrick and Refractories).
  2. Make retorts: closed-ended tubes or long pear shapes 25–35 cm long and 8–12 cm across, with walls 1–1.5 cm thick, open at one end.
  3. Make condensers: tubes 15–20 cm long with a bore of 2–3 cm, which fit snugly into the retort mouths.
  4. Dry them for a week; fire them in the The Kiln.

The furnace

Build a furnace of brick or stone and clay with two chambers, one above the other, separated by a thick fired-clay plate about 5–8 cm thick, pierced with holes just large enough for the condensers:

  • the upper chamber, where the retorts stand mouth-down with their bodies surrounded by fuel and the full blast — this must reach 1,100–1,200 °C, a full yellow to yellow-white;
  • the lower chamber, where the condensers poke through, kept much cooler — a dull red at most, so that zinc condenses as a liquid (above 420 °C, below about 900 °C). Openings in its walls let you reach in and let heat out.

The run

  1. Charge each retort with roasted, powdered ore mixed with about half its weight of charcoal powder, moistened so it holds together. Fill to within 3 cm of the mouth.
  2. Fit the condenser into the mouth and seal the joint with fireclay. Push a loose plug of dry grass or a perforated clay disc into the top of the condenser first, so the charge cannot fall down it.
  3. Set the retorts mouth-down through the holes in the plate, condensers projecting into the lower chamber. Put a small clay cup under each condenser.
  4. Fire the upper chamber with charcoal and a good blast. Raise the heat steadily over 2 hours to yellow, then hold it for 4–6 hours.
  5. Watch the condensers. Zinc vapour passes down them and condenses: drops of bright liquid metal run out into the cups. A small blue-white flame at a condenser tip is a little zinc burning — normal. Clouds of white smoke from a condenser mean it is too hot or cracked; a condenser choked with grey powder ("blue powder", fine unmelted zinc) is too cold.
  6. Cool, then collect the zinc from the cups. Remelt it at about 450–500 °C under a little charcoal and cast it into plates. Break the spent retorts out of the plate; most are used once.

Note The Chinese method stands the retorts the other way up: tall clay jars packed in coal, with a condensing pocket sealed onto the top of each. Zinc vapour rises into the cooler pocket and collects on a shelf. Either arrangement works; what matters is no air, a hot charge and a condenser in the right temperature range.

A run of a dozen small retorts can yield a kilogram or two of zinc. Losses are large at first — half the zinc may escape as smoke or stay in the residue. That is normal.

Method 3: Making and using brass and zinc

Brass from zinc metal. Melt copper in a crucible under charcoal (see Copper Smelting). Warm the zinc beside the furnace, then drop it in and stir with a dry stick. It will flare and smoke — add it in pieces, keep the charcoal cover on, and pour within a minute or two. Add 5–10% extra zinc to make up for what burns.

Brass Copper : zinc Use
Gilding metal 85 : 15 Gold-coloured, soft; ornaments, badges, plating base
70/30 brass 70 : 30 The best for cold work: drawing wire, deep-pressed sheet, tubes, springs
Yellow brass 63–65 : 35–37 General castings and sheet
60/40 (Muntz) brass 60 : 40 Casts and hot-forges well; ship sheathing, taps, valves, bolts
Brazing spelter 50 : 50 Melts about 870 °C; a filler for joining iron, copper and brass

Pour brass at 1,000–1,050 °C (orange-yellow). Like copper, brass work-hardens and is annealed by heating to a dull red. Wire is drawn exactly as copper wire is (Copper Wire).

Zinc plates and sheet. Cast zinc plates for batteries in iron or stone moulds. Cold zinc is brittle and cracks when bent, but between 100 and 150 °C — when a drop of water hisses and dances on it — it becomes soft and can be hammered or rolled into sheet. Above about 200 °C it goes brittle again.

Galvanising iron.

  1. Clean the iron by pickling in dilute acid (see Sulfuric Acid or Hydrochloric Acid) and scrubbing with sand until it is bright.
  2. Dip it in a flux: zinc dissolved in hydrochloric acid until no more fizzing occurs (zinc chloride), with a little sal ammoniac if you have it. Dry it on a warm stone.
  3. Dip it into molten zinc at about 450–460 °C (just hot enough that a dry pine shaving chars at once) for a minute or two, until the bubbling stops. Lift it out slowly and shake off the excess.

The zinc bonds to the iron as a grey, spangled coat that protects it for decades, even at scratches, because the zinc is eaten instead of the iron (see Corrosion and Its Prevention).

How to tell it worked

  • Brass is golden yellow, never pink; filed, it shows a yellow, brassy surface. It is harder and springier than copper, and does not pull toward a lodestone. The more zinc, the paler and yellower it is.
  • Zinc is bluish-white with a crystalline, spangled break. It is about seven times as heavy as water. A strip dropped in vinegar or dilute acid fizzes steadily (hydrogen) — copper and brass do not. Bent cold, it creaks and cracks.
  • Battery test: a zinc plate and a copper plate in salty water give a current that swings a galvanoscope (The Battery).

Note Troubleshooting. Cementation copper came out pink, no weight gain → too cold, too short, or air got into the crucible. Seal better; hold longer at cherry-orange; finer copper. Huge white smoke during cementation → too hot too early. Hold below copper's melting point until the vent flame dies. No zinc from the retorts, only white powder in the lower chamber → condensers too hot, cracked, or leaking air. Check every joint; shade the lower chamber. Condensers full of grey powder → too cold. Close up the lower chamber openings a little. Zinc cracks when bent → normal when cold. Work it at 100–150 °C. Brass casting full of holes → zinc boiled in the melt. Don't overheat; pour as soon as it is fluid.

Dangers

Danger Metal fume fever. Breathing white zinc oxide smoke — from cementation, distillation, melting brass, or galvanising — brings on fever, shivering, aching muscles, a sweet metallic taste, headache and a cough, 4 to 12 hours later. It usually passes in a day or two, but repeated attacks harm the lungs. Work outdoors, upwind, and never breathe the white smoke.

Danger Cadmium and lead. Zinc ores often contain cadmium, which boils even lower than zinc (767 °C) and comes off first, as a brownish fume. Cadmium fume can inflame the lungs fatally a day after exposure, and slowly destroys the kidneys and bones. Zinc ores also carry lead. Distil and melt only with the wind at your back, keep everyone else well away, and do not eat or drink near the work. Keep apart the first zinc that runs from each retort, which is the richest in cadmium, and never use it for anything that touches food.

  • Sulfur dioxide from roasting sphalerite: roast in the open, upwind (see Lead).
  • Acids used for pickling and flux: see Acids, Bases and Testing.
  • Never use zinc or galvanised vessels for acid food: zinc dissolves into it and causes vomiting.
  • Molten metal and water: dry moulds, dry ground, dry tools, as always.

What this unlocks

Zinc and copper make the voltaic pile and the Daniell cell (The Battery), and from them Electrolysis, the The Electromagnet and the The Telegraph. Galvanised iron gives you rust-proof wire, buckets and roofing (Roofs). Brass gives you clock wheels, screws, pins, instrument parts and valves — the parts of clocks, compasses, barometers and the The Steam Engine. Zinc chloride is the classic flux for Soldering and Brazing, and brass spelter is the filler for brazing.

How it was first done

Small amounts of brass appear in the Near East from the first millennium BC, probably made by accident from mixed ores. The Romans made brass deliberately by cementation from about the 1st century BC, and from the reign of Augustus they struck coins of it, called orichalcum. Cementation remained the only way to make brass in Europe until the 18th century.

Zinc metal was first made on a large scale in India. At Zawar in Rajasthan, smelters distilled zinc downward in thousands of small clay retorts; production there was under way by about the 9th century AD and was large by the 14th, leaving huge heaps of spent retorts. In China, zinc was being distilled by the 16th century, and Song Yingxing described the process in his book Tiangong Kaiwu (1637). Chinese zinc was shipped to Europe as "spelter" in the 17th century. In England, William Champion patented a downward-distillation process in 1738 and built zinc works near Bristol, and in Germany Andreas Marggraf described making zinc from calamine in 1746. In 1805 two Sheffield makers found that zinc becomes workable when warmed, which made sheet zinc possible, and in 1837 the Frenchman Stanislas Sorel patented hot-dip galvanising.