Part 5 · Cloth and Clothing
Elastic and Rubber Thread
Thin threads of cured rubber, cut from sheet or squirted from latex, wrapped in cotton and woven, knitted or braided into tapes and cords that stretch and spring back. They hold up trousers and stockings, close cuffs, make rubber bands, and give doctors firm, even bandages and stockings for injured and swollen legs.
- Difficulty
- ●●●●●
- Time
- A day to cut thread from a cured sheet; an afternoon to cover a few metres by hand; a day to weave 2 m of webbing on a band loom
- Steps from zero
- 5 prerequisites →
This unlocks
—The full path from nothing — 5 steps before this one
- Cordage and Rope
- Sulfur
- Spinning and Weaving Cloth
- Rubber
- Tablet and Band Weaving
- Elastic and Rubber Thread
Do them roughly in this order. See it on the tech tree →
Why it matters
Cloth stretches only a little and does not spring back. To make clothing that grips the body without buttons, laces or tight belts — a waistband, a sock top, a cuff, a hat strap — you need something that pulls back like a muscle. Rubber thread does it, and once it is wrapped in cotton and woven into a tape it lasts for years of washing and wear.
Elastic also matters in medicine. An elastic bandage holds a sprained ankle with steady, even pressure. A compression stocking squeezes the leg most at the ankle and less higher up, pushing blood back towards the heart; it heals and prevents the leg ulcers of varicose veins, which otherwise cripple many older people. And the humble rubber band holds bundles of everything together.
This chapter starts from cured soft rubber as made in Rubber and uses the narrow looms of Tablet and Band Weaving and the needles of Knitting, Crochet and Netting.
How it works
Rubber is a tangle of long, coiled chains. Pull it and the chains straighten; let go and their jiggling heat-motion coils them back up. Vulcanising with sulfur ties the chains together so they cannot slide past each other, so the rubber returns to its exact shape (Rubber). Good soft rubber stretches to 5–7 times its length before breaking.
Bare rubber thread has three faults: it grips and drags on skin and cloth, it is weakened by sunlight, oil and sweat, and it can be stretched until it snaps. Covering solves all three. A cotton or silk yarn is wound round the thread while the rubber is stretched. When the rubber relaxes, the yarn bunches into loose coils. The covered thread can now stretch only until the yarn coils are pulled straight — about as far as it was stretched while being covered — and then the yarn takes the load. The cotton also feels like cloth, takes dye and shields the rubber.
In elastic webbing, covered rubber threads lie inside a woven tape, also stretched. When the tape relaxes, the rubber pulls the cloth into tiny ripples. Stretch the tape, and it extends until those ripples are flat.
What you need
| For | Item | Notes |
|---|---|---|
| Cut thread | Cured soft rubber sheet, 0.5–1 mm thick; a The Lathe or a cutting board | Soft-rubber recipe in Rubber, with little or no filler |
| Extruded thread | Fresh or ammonia-preserved latex, fine sulfur, a funnel with a glass tip, a long trough, vinegar | Ammonia, vinegar |
| Covering | Fine cotton or silk yarn, a serving tool or covering spindle | Spinning and Weaving Cloth, Silk |
| Webbing | Inkle loom or band heddle, cotton or linen warp and weft | Tablet and Band Weaving |
| Bands | Glass or glazed clay rods, or smooth hardwood dowels | Glass, Pottery |
| Curing | Iron box, sand or chalk, a slow fire | As in Rubber |
Rubber thread
Rubber thread for clothing is 0.4–1.2 mm across. Finer threads make soft, gentle elastic (stockings, cuffs); thicker ones make strong elastic (waistbands, bandages).
Method 1: Cut thread
The first rubber thread was cut from sheet, and it is still the easiest route with no special tools.
By hand. Roll a sheet of compounded but uncured soft rubber to an even 0.8 mm between two boards on guide strips of that thickness (Rubber), dust it with chalk and cure it flat. Lay the cured sheet on a smooth hardwood board and wet it with soapy water so the blade glides. Hold a steel straightedge on it with a spacer strip 0.8–1 mm wide against the sheet's edge, and draw a very sharp knife along it in one stroke. Move the straightedge across by the spacer's width and repeat. You get square threads as long as the sheet. Join lengths by scarfing the ends at a long slant, painting them with rubber cement and binding them with fine thread; better still, make the sheet long.
On a lathe (better). This gives hundreds of metres in one piece.
- Wrap uncured sheet once round a smooth wooden or metal drum, say 30 cm across (about 1 m round) and 50 cm long, with a narrow cemented overlap. Wrap it with a spiral of wet cloth tape and cure it on the drum.
- Mount the drum in a lathe with screw-cutting gears or a lead screw (The Lathe, Screws, Nuts and Bolts). Set a thin, very sharp blade square to the rubber, just deep enough to cut through it, and set the carriage to move 1 mm sideways per turn.
- Run the lathe slowly with water dripping on the cut. The blade slits the sheet along a helix, peeling off one continuous thread about 1 m long per turn — 500 m from a 50 cm drum.
A cut thread has a square section and slightly rough edges. It is good enough for all covered work.
Method 2: Extruded latex thread
Liquid latex squirted through a fine nozzle into acid sets into a smooth, round, seamless thread, as long as you like. It needs liquid latex, so it suits places where rubber trees or latex plants grow.
- Preserve and strain. Stir about 20 ml of strong ammonia water per litre of fresh latex (roughly 0.5% ammonia) (Ammonia) to stop it setting, and strain it through fine cloth.
- Compound. Grind fine sulfur with a little water and a pinch of soap on a stone slab for an hour into a smooth cream. Stir in about 2 g of sulfur per 100 g of rubber in the latex (latex is roughly one-third rubber). Add a little fine zinc white if you have it (Zinc and Brass); it helps the cure. Let it stand 1–2 days in a covered pot, stirring now and then.
- Extrude. Fill a raised funnel or pot with a glass nozzle of 0.6–1 mm bore at the bottom. Let the latex run in a steady stream into a long trough of strong vinegar, at least 2 m long. Where it enters the acid, it sets into a soft, white jelly thread. The stronger the acid, the faster it sets: vinegar concentrated by freezing out some of its water works better than plain vinegar, and a longer trough gives the thread more time. Lead it along the trough and pull it out at the far end onto a slowly turning reel. The speed of pulling sets the thickness: pull slowly for thick thread, faster for fine. Several nozzles side by side make several threads at once.
- Wash and dry. Run the reel of thread through clean water to wash out the acid, then dry it in warm, shaded air for a day, dusted with chalk so it does not stick to itself.
- Cure in the sand box at 130–150 °C for 1–2 hours, judged with a pinch of sulfur as in Rubber.
Without the chemical helpers (accelerators) of modern industry, the cure is slow and must be watched; test samples at intervals.
Testing thread
- Stretch a 10 cm piece to 50 cm (5 times). It must not break, and when released it must come back to within about 11 cm in a minute.
- Heat a piece a day on a sunny stone: it must not go sticky. Cold: a night on ice and it still bends without cracking.
- Old age: hang a stretched piece in sunlight for a week. Fine surface cracks across it mean too little sulfur or overcuring; it will not last.
Covered elastic thread
By hand: serving. Tie one end of a 1–2 m length of rubber thread to a fixed hook. Stretch it to 3 times its relaxed length and tie the other end to a second hook. Wind fine cotton or silk yarn on a small bobbin. Tie the yarn to the thread at one end and pass the bobbin round and round the rubber, close and even, laying the turns side by side as you walk slowly along — just as a rope's end is bound with twine (Ropewalks and Sailcloth). About 10–15 turns per centimetre of stretched thread is right for yarn 0.2–0.3 mm thick. Tie off and release. For a smooth, balanced thread that does not twist, cover it a second time in the opposite direction (double covering).
Covering spindle (better). The rubber thread runs up through the middle of a hollow spindle — a tube with a 3–4 mm bore and a whorl, driven by a band from a spinning wheel (The Spinning Wheel) or a treadle at 1,000 turns a minute or more. A bobbin of yarn sits on the spindle and whirls round with it. The yarn unwinds from the bobbin and wraps itself round the rubber as it passes up out of the top. Feed the rubber from a reel with a light brake so it arrives stretched about 3 times, and pull the covered thread off onto a take-up reel turned at a steady speed. The ratio of spindle speed to take-up speed sets the turns per centimetre.
Uses. Covered elastic thread is shirring elastic: wound on the bobbin of a The Sewing Machine (or sewn by hand in rows of small running stitches), it gathers cloth into stretchy rows for the bodices and cuffs of children's clothes. Laid in with the yarn on ribbed knitting, it tightens cuffs and sock tops.
Elastic webbing
Woven elastic is the strongest and flattest elastic tape: for waistbands, braces (Buttons, Buckles, Hooks and Zips), garters and bandages.
- Plan the tape. For a waistband 25 mm wide: 8 covered rubber ends, with 2–3 ground ends of fine cotton or linen between each pair of rubber ends and at both edges — about 30 ground ends in all.
- Warp the loom. Use a band heddle with a backstrap, or an inkle loom set up with a straight warp from a fixed post (Tablet and Band Weaving). Warp the ground ends normally, alternating heddled and open.
- Add the rubber. Cut each rubber end half the length of the ground warp and tie both ends to the same anchors as the ground warp, so that under weaving tension the rubber is stretched to about twice its length. The rubber ends do not pass through heddles or slots. Lead them through a reed, a comb or a card with holes to keep them in order, at the height of the middle of the shed.
- Weave. Open the first shed. Pass the weft above all the rubber ends (between the upper ground threads and the rubber). Change the shed and beat. Pass the next weft below all the rubber ends. Repeat: over, under, over, under. Each rubber end ends up inside a little sleeve of woven cloth. Beat firmly; aim for 10–14 picks per centimetre.
- Release. Cut the tape off and let it relax. It should shrink to about half its woven length and gather into fine even ripples.
Knitted elastic. In single rib (knit 1, purl 1, Knitting, Crochet and Netting), carry a covered elastic thread along with the yarn, or lay it in behind the purl stitches every second row. Ribbed cuffs, sock tops, compression stockings and soft waistbands are made this way. Knitted elastic is softer and kinder to skin than woven.
Braided elastic and elastic cord. Braid cotton yarn round a core of several stretched rubber threads with an 8-strand round braid (Cordage and Rope). A braid over 3–6 rubber threads makes round elastic cord, 2–4 mm thick, for hat straps, masks and bag closures; a thick core of 50–200 threads with a tough braided cover makes shock cord for tents and loads (Tents, Sleeping Bags and Camping Gear). Braided elastic narrows when stretched, so it suits casings, not flat bands.
A good elastic tape is the same width all along, the ripples are even, it stretches to 1.5–2 times its relaxed length and comes straight back, and no rubber shows at the edges.
Rubber bands
A rubber band is a ring sliced from a rubber tube (Envelopes, Stamps, Clips and Office Supplies).
- Make the tube. Simplest: wrap uncured compounded sheet 1 mm thick once round a greased glass, glazed-clay or hardwood rod with a narrow cemented overlap. Bind with wet cloth tape and cure. Seamless (better): dip a clean glass or glazed rod into compounded latex (as for extruded thread), lift it out, let it dry 10 minutes, and dip again 4–6 times until the coat is about 1 mm thick. Dry for a day and cure on the rod.
- Slice. Slide the tube off (soapy water helps), put it back on a dry wooden rod, and slice rings with a sharp wet knife against a guide block. Ring widths of 1.5–6 mm.
- Sizes. A useful general band is about 3 mm wide, 1 mm thick and 7–9 cm long laid flat, cut from a tube about 5 cm across. Wider and thicker bands hold harder.
Testing: a good band stretches to 5–6 times its flat length without cracking and returns to within 5%. Bands that turn sticky or crack were undercured or overcured; old bands perish in sunlight and near copper, oil or grease.
Uses in clothing
- Waistbands. Sew a channel (casing) along the top of a garment 5 mm wider than the elastic. Cut the elastic to 85–90% of the body measurement, thread it through with a safety pin (Buttons, Buckles, Hooks and Zips), overlap its ends 2 cm and sew them in a square with a cross. For a shaped, flat waist, sew the elastic straight to the cloth, stretching it as you stitch.
- Garters. A band of elastic webbing 2–2.5 cm wide, sewn into a ring that fits snugly round the leg, or fixed to a stocking top with a clip. Make them firm, not tight.
- Cuffs, sock tops, hats and underwear use knitted or narrow woven elastic, 6–15 mm wide.
- Elastic-sided boots have a gusset of strong woven elastic set into each side, so they pull on without laces (Footwear).
Uses in medicine
Elastic bandage. Weave webbing 7.5–10 cm wide with fine covered rubber threads every 3–4 mm across the width, or knit it in rib. It should stretch to about twice its length. To support a sprained ankle: start at the base of the toes, wind round the foot and then up the leg in a spiral, each turn covering half the one before, stretched to about half of its full stretch. Check the toes afterwards — see Dangers. See Wound Care and Antiseptics and The First Aid Kit.
Compression stocking. For varicose veins, healed leg ulcers and swollen legs. Knit a stocking in rib to the person's measurements, with covered elastic laid in, firmest at the ankle, a little looser at the calf and loosest below the knee. Measure the ankle at its narrowest and the calf at its widest first thing in the morning, before swelling, and knit the stocking a little smaller than those measurements — roughly 10% smaller to start with. Try it on: it should feel firm but comfortable, with toes that stay pink and warm (see Dangers); make the next one tighter or looser to suit. Put it on before getting up, remove it at night. It must never be tighter at the top than at the ankle.
How to tell it worked
- Stretch and return: elastic, thread and bands go back to within a few percent of their length after a minute.
- Washing: a test piece washed in warm soapy water 20 times keeps its spring. Hot water, bleach and boiling shorten its life (Laundry and Bleaching Cloth).
- Months of wear: good elastic stays springy for a year or more of daily use.
Note Troubleshooting. Thread sticky → undercured. Cure longer. Thread breaks easily or cracks when stretched → overcured, too much filler, or air bubbles. Use less chalk, cure cooler. Covered thread twists and kinks → single covering is unbalanced; double cover in the opposite direction. Webbing uneven, some ripples deeper than others → rubber ends not stretched equally; measure each to exactly half length. Rubber poking out of the tape → too few picks per centimetre, or the weft not alternating over and under the rubber. Elastic gone limp after months → overheating in washing or drying, or sweat and grease. Wash cool, dry in shade.
Dangers
Danger Tight elastic can cut off blood flow. A bandage, stocking or band wound too tightly round a limb, finger or neck can kill tissue within hours. After applying any elastic bandage, the toes or fingers must stay pink and warm; press a nail and the pink must return within 2 seconds. Numbness, tingling, cold, blue or white skin, or growing pain mean unwind it at once. Never use elastic as a tourniquet; use a proper strap only as Wound Care and Antiseptics directs. Never put rubber bands or tight elastic on babies or children, and keep bands away from them — they can be swallowed or choke.
- Eyes. A snapping band or a broken stretched thread can injure an eye; do not stretch elastic near your face.
- Latex allergy. Some people react to rubber with itching rashes, and a few with wheezing and collapse. Use covered thread, keep rubber away from their skin, and never use rubber gloves or bandages on someone known to react.
- Curing fumes and ammonia. Curing gives off hydrogen sulfide, and preserved latex gives off ammonia; work outdoors (Rubber).
- Compression stockings are dangerous for people whose legs have poor arterial blood flow — cold, pale feet, weak pulses, or pain in the calf when walking. Have such people checked before using them (Examining a Patient).
What this unlocks
Elastic finishes clothing (Making Clothes, Tailoring and Pattern Drafting), makes braces, slings and support garments, and gives Crutches, Prosthetics and Rehabilitation and Hearing Aids, Braille and Daily-Living Aids straps that hold without buckles. Shock cord secures loads and tents, and thick rubber cords launch gliders and power model aircraft and toys (Toys). The same stretched-core covering method makes strong composite yarns, and the latex-dipping method makes balloons, gloves and teats (Nappies, Feeding Bottles and Baby Gear).
How it was first done
The peoples of Mesoamerica made rubber bands and sandal straps long before Europeans arrived (Rubber). In England, Thomas Hancock patented elastic fastenings for gloves, shoes and stockings in 1820, cutting thin strips from raw rubber bottles brought from South America; to use up the waste he invented his masticator. Elastic-sided boots were made in the 1830s by the London bootmaker Joseph Sparkes Hall. Raw rubber went soft in heat and hard in cold, so elastic only became reliable after vulcanisation (Goodyear and Hancock, 1839–1844); Stephen Perry patented rubber bands in 1845, and woven elastic webbing for braces and garters became a large industry in Britain and the United States in the following decades. Extruded latex thread came in the 1920s, and covered latex yarn sold as "Lastex" from 1931 made close-fitting swimsuits and foundation garments possible. In 1958 Joseph Shivers at DuPont made spandex (elastane), a fully synthetic elastic fibre that has largely replaced rubber thread in clothing (Rayon and Nylon), though rubber thread is still used where strong pull is needed.