Part 2 · Earth and Fire
Pyrometric Cones and Kiln Temperature
Slender clay pyramids that bend over at a known heat tell you what your pots have actually felt in the kiln. How to make a numbered series of cones and calibrate it, set a cone pack, pull draw rings, read shrinkage rings, judge heat by colour, fit a thermocouple, build a disappearing-filament optical pyrometer, and write firing schedules that come out the same every time.
- Difficulty
- ●●●●●
- Time
- A day to make a year's cones; one calibration firing; an afternoon per draw-ring set; a week to build and calibrate an optical pyrometer
- Steps from zero
- 8 prerequisites →
This unlocks
—The full path from nothing — 8 steps before this one
- Fire
- Finding and Preparing Clay
- The Kiln
- Pottery
- Lime
- Lye and Potash
- Glass
- Glazes
- Pyrometric Cones and Kiln Temperature
Do them roughly in this order. See it on the tech tree →
Why it matters
A potter who fires "by eye" can make good pots but cannot repeat a firing that went well, or teach anyone else to. A glaze glossy one week comes out dry and pinholed the next. Twenty degrees decide between a stoneware jug that rings and holds water and one that slumps on the shelf (Stoneware and Porcelain).
This chapter gives you numbers you can write down. A row of small clay cones, made once from your own glaze materials, tells you when to stop firing. Rings pulled from the kiln show what the glaze is doing now. A thermocouple shows how fast the heat is climbing, and an optical pyrometer reads the heat of a furnace, a pour of molten metal or a glass tank from across the room. Together they turn the The Kiln from an art into a process that any trained worker can repeat, which is what a pottery factory (Slip Casting, Jiggering and Ceramic Factories), a brickworks (Bricks), a cement plant (Portland Cement) or a glassworks (Glass) needs.
How it works
Heat-work, not temperature. Clay and glaze do not change the moment they reach a temperature. Melting, sintering (grains welding together) and glaze maturing all take time. A glaze that needs 1,240 °C when heated quickly may mature at 1,220 °C if held there for an hour. What the ware feels is the combination of temperature and time, called heat-work.
A pyrometric cone (from Greek pyr, fire) is a small, slender pyramid of glaze-like material. As heat-work builds up, it softens and bends over under its own weight, exactly as a glaze softens and flows. Because it responds to time as well as temperature, it measures what the pots feel, not just how hot the air is. Cones are made in a numbered series, each one needing a little more heat-work than the last. Rated cones bend about 20 °C hotter when heated at 150 °C an hour than at 60 °C an hour.
The ingredients decide the bending point. Fluxes (potash, soda, lime from feldspar, glass and limestone) make a mixture melt; alumina and silica (from kaolin and quartz) stiffen it. Hermann Seger made his standard series by keeping the fluxes the same and raising the alumina and silica together, step by step. You will do the same with what you have.
Glowing colour. Everything hot enough glows, and the colour depends only on the temperature: dull red near 600 °C, orange near 1,000 °C, yellow-white above 1,200 °C. The table is in The Kiln and The Thermometer. The optical pyrometer sharpens this into a measurement by comparing the glow with a lamp filament whose brightness you control and have calibrated.
Thermocouples. Two different metal wires joined at a hot tip give a small voltage that rises with temperature (Thermocouples and Thermoelectricity). They read the air at one point, continuously, which is ideal for watching the rate of climb but not what the ware feels.
What you need
| Item | For | Notes |
|---|---|---|
| Ground glaze materials | Cones | Feldspar, kaolin, quartz, limestone, bottle glass; all through the finest sieve (Glazes) |
| Dextrin or gum arabic | Cone binder | Dextrin is starch toasted until it turns tan (Glues and Adhesives) |
| A cone mould | Cones | Split plaster or brass, a three-sided pyramid cavity (Gypsum and Plaster of Paris) |
| Grogged clay | Cone plaques, rings | Your normal kiln clay with 20–30 % grog (Firebrick and Refractories) |
| Sentinels | Calibrating | Pure silver, gold, copper; salt (The Thermometer) |
| Thermocouple and millivoltmeter | Rate of climb, calibration | Thermocouples and Thermoelectricity, Measuring Electricity |
| Iron rod 1.5 m long with a hooked end | Draw rings | Blacksmithing |
| Dark glass | Eyes | Welding glass or smoked glass; cobalt-blue glass |
| Lenses, a small lamp, a rheostat, an ammeter | Optical pyrometer | Lenses, The Light Bulb, Measuring Electricity |
Where to find it
The cone materials are the glaze materials of Glazes and Stoneware and Porcelain: feldspar (the pink or white blocky crystals of granite), kaolin (white china clay from rotted granite), quartz (crushed vein quartz or clean white sand), limestone (fizzes with vinegar) and powdered bottle glass (Glass). Grind them to flour and sieve them through the finest silk you have.
The one rule that matters: make each mixture in a large batch from a single lot of materials, enough for years. Feldspar from one pit differs from the next. Your calibration holds only for that batch.
Making pyrometric cones
The series
Make two series of mixes by dry weight. Number them in order; the numbers are your own.
| Cone | Mix | Where it falls |
|---|---|---|
| L1 | Bottle glass 100 | Lowest: about dull cherry red |
| L2 | Bottle glass 90, kaolin 10 | |
| L3 | Bottle glass 80, kaolin 20 | |
| L4 | Bottle glass 70, kaolin 30 | Bisque and earthenware range |
| L5 | Bottle glass 60, kaolin 40 | |
| H1 | Feldspar 60, bottle glass 40 | Hard earthenware, start of stoneware |
| H2 | Feldspar 75, bottle glass 25 | |
| H3 | Feldspar 90, limestone 10 | |
| H4 | Feldspar 100 | Stoneware |
| H5 | Feldspar 90, kaolin 10 | |
| H6 | Feldspar 80, kaolin 20 | Porcelain range |
The right-hand column is only a rough guide. Pure bottle glass bends somewhere around 700–800 °C and pure potash feldspar near 1,250–1,300 °C; the mixes in between fall in order, but only calibration gives you their numbers. If two neighbouring cones go down together, make an in-between mix; if a gap is too wide, add a step.
Shaping
- Weigh 200 g of each mix. This makes about 40 large cones.
- Bind: stir 5 g of dextrin into 25 ml of hot water and work it into the powder until it is like damp sand that holds together when squeezed. A trace of red iron oxide or charcoal powder in one series makes the two series easy to tell apart, as long as it is in the batch you calibrate.
- Press it hard into the mould with a wooden tamper. The standard large cone is 6.4 cm tall with a triangular base 1.6 cm on each side; a small cone for a kiln switch is 3 cm tall (Thermostats and Automatic Control).
- Open the mould and slide the cone out onto a board. Scratch its number on one face with a pin.
- Dry for two days. Store in labelled, dry boxes. Do not fire them first.
Calibrating
- Set one cone of every number in a row of plaques where you can see them through a spy hole. Put a thermocouple tip right beside them (Thermocouples and Thermoelectricity) and, on a fired-clay tray beside them, small pieces of pure silver (melts at 962 °C), gold (1,064 °C) and copper (1,085 °C) and a crystal of salt (801 °C). Bury the copper in a pinch of charcoal in a small lidded dish: in open kiln air it oxidises and melts early, at about 1,065 °C.
- Fire at a steady 60 °C an hour over the last 200 °C. Watch through dark glass and note the reading and time as each cone's tip bends level with its base, and as each sentinel melts.
- Write the results in your kiln book as a table: cone number, temperature at 60 °C an hour. Repeat with a second firing to check; cones from one batch should agree within 5–10 °C.
Good or bad: a good cone is crisp-edged, hard when dry, bends smoothly in a gentle curve and ends glassy. A cone that bloats, leans before it softens, or slumps all at once into a puddle is badly mixed or too coarse. One that cracks or falls over was set loosely or pressed too dry.
Setting a cone pack
A cone pack is a plaque holding three cones:
- Guide cone: one number below the target. When it bends, you are close; slow down.
- Firing cone: the target. When its tip is level with its base, the firing is done. Begin the soak or shut down.
- Guard cone: one number above. If it bends too, you have overfired.
Make the plaque from a pad of grogged clay 2 cm thick. Push each cone 1 cm deep, leaning 8° from upright, all leaning the same way, with the numbered face toward the lean, 2 cm apart so they do not fall on each other. Let the plaque dry before firing. Put packs where you can see them through the spy holes, out of the direct flame, and one at the top and bottom of the kiln: if all go down within one number of each other, the kiln is even.
Draw rings
A draw ring (draw trial) is a small piece of ware that you pull out of the kiln during the firing to see what is actually happening.
- Make rings of your clay body 4–5 cm across, 1 cm wide, 5 mm thick. Glaze them as the ware is glazed.
- Set a row of them on a shelf or stand right behind a spy hole, each standing on edge so a hook can catch it.
- Draw: near the end of the firing, hook one out with the long iron rod. Lay it on a brick to cool, or drop it in a bucket of water to cool it in seconds (stand back: it spits).
- Read: a mature glaze is smooth and glossy, with no pinholes or rough patches; an underfired one is dull, rough and pitted. Break the ring: the body should be dense, with no white chalky core. Salt-glaze potters draw one after each throw of salt to judge the glaze (Glazes).
Temperature rings
A temperature ring is a pressed disc of a carefully made clay mixture that shrinks more the more heat-work it gets. Wedgwood used small clay cylinders slid along a tapering brass groove in 1782; later works used rings measured on a gauge (Buller's rings). Their great virtue is that you can read them after the firing, in any light, and file them in the kiln book.
- Mix a large batch of a fine, even body: for example kaolin 50, plastic clay 30, quartz 20, sieved and well mixed. As with cones, one batch for years.
- Press rings in a steel or plaster ring mould: 6 cm across, 1 cm thick, with a 1.5 cm hole. Dry them.
- Fire one ring in each of several kiln positions.
- Measure the fired diameter with calipers to 0.1 mm (Rules, Squares, Callipers and Gauges), or on a gauge: a flat plate with a fixed stop and a pivoted pointer 20–30 cm long whose short arm, 2–3 cm, rests against the ring. The pointer magnifies the shrinkage ten times on a scale at its tip.
- Calibrate by firing rings with cones and a thermocouple; a 1 mm difference in diameter typically corresponds to some tens of degrees.
Reading the colour of heat
The colour table in The Kiln is good to about ±50 °C if you always look in the same dim light (in sunlight a kiln looks 100 °C cooler), look at the ware and far wall rather than the flames, and switch to watching cones through dark glass above about 1,150 °C, where everything is too bright to judge. Train your eye by naming the colour aloud and then checking the thermocouple; after a dozen firings most people are within 30 °C.
Thermocouple pyrometers
The thermocouple and how to make and calibrate one are in Thermocouples and Thermoelectricity. For a kiln:
- Iron and constantan (copper–nickel) wire works to about 700 °C, enough for bisque; nickel–chromium against nickel–aluminium (type K) to about 1,250 °C; platinum against platinum with 10 % rhodium (type S) to 1,450 °C.
- Put the hot tip 3–5 cm inside the chamber, through a hole in the wall, in a closed-end porcelain or alumina tube. Keep it out of the flame path; flames read hot.
- Read every 15–30 minutes and plot temperature against time on squared paper. The slope is your rate of climb, the number every firing schedule is written in.
- A thermocouple reads the air; the ware lags behind, and holds the heat-work. Trust the cones for when to stop; trust the thermocouple for how fast to go. Check one against the other every few firings.
The optical pyrometer
An optical pyrometer reads the temperature of anything glowing, from a distance, without touching it: the inside of a kiln, a stream of molten iron, a glass furnace, a steel bar in the forge. It works from about 700 °C to 1,400 °C as built here, and far higher with a dark glass added.
How it works. A small telescope looks at the hot object. Inside it, exactly where the lens forms the image of the object, hangs a lamp filament. Looking through the eyepiece, you see the filament as a dark line against the glow. Turn up the lamp current: the filament brightens until it vanishes against the background, then shows as a bright line. At the vanishing point the filament is exactly as bright as the object. A red filter in the eyepiece makes both the same colour, so you compare only brightness, which the eye does very precisely: to within about 5–10 °C.
Building one.
- Tube: brass, wood or stiff card, 30–40 cm long, 3–4 cm across, blackened inside with soot and glue.
- Objective: a lens of focal length 20–25 cm, 2–3 cm across, at the front (Lenses). Behind it, a stop with a 1 cm hole cuts stray light.
- Lamp: a small vacuum lamp with a single straight or hairpin filament of carbon or tungsten (The Light Bulb), mounted so the filament sits in the plane where the objective focuses an object 1–3 m away. Slide it back and forth until a distant glowing object and the filament are sharp together.
- Eyepiece: a lens of focal length 2–3 cm that focuses on the filament (The Telescope).
- Red filter: a disc of copper-ruby glass (Glass) between eyepiece and eye.
- Circuit: a 2–4 volt battery (The Rechargeable Battery), a sliding-wire rheostat for fine control, and an ammeter in series (Measuring Electricity). The lamp will want somewhere between a fifth of an amp and an amp, depending on its filament.
Calibrating. The pyrometer must look into something that glows as a perfect radiator, a blackbody: a hole into a closed hot cavity. Push a fireclay tube closed at the far end deep into a crucible of molten metal, and sight into the tube. As the metal cools and freezes, its temperature stands still for minutes (Thermocouples and Thermoelectricity): pure silver at 962 °C, gold at 1,064 °C, copper at 1,085 °C (copper only under a layer of charcoal, which keeps it from oxidising). Note the vanishing current at each. Add points from a calibrated thermocouple in a kiln up to 1,300 °C. Draw a smooth curve of current against temperature and fix it inside the lid of the pyrometer's box.
Using it. Sight into the kiln, through a spy hole at the far wall or the ware, where conditions are close to a blackbody. An open bright surface outside a furnace, such as a stream of molten iron or a white-hot bar in air, reads 50–150 °C too low, because shiny hot surfaces glow less than a hole into a cavity at the same heat. Note on each reading what you looked at.
Going higher. A piece of smoked or grey glass between the objective and the lamp cuts the brightness by a fixed amount. Calibrate it once against the plain instrument at overlapping temperatures, and the same lamp then reads steelmaking and arc-furnace heat (The Electric Arc Furnace).
Firing schedules
A firing schedule is the plan of rates and holds, written in degrees an hour. Here are three to start from; change one thing at a time and log every firing.
Bisque (first firing), to about 950 °C.
| Stage | Rate | Why |
|---|---|---|
| Room heat to 200 °C | 50 °C an hour (slower for thick ware) | Drive out water without bursting pots |
| 200–600 °C | 100 °C an hour | Burn out carbon; pass the quartz change at 573 °C gently |
| 600–950 °C | 150 °C an hour | |
| Hold | 20–30 minutes, until the bisque cone is down | Even heat |
| Cool | Naturally; open below 200 °C |
Earthenware glaze, about 1,050–1,120 °C. 100 °C an hour to 600 °C; 150 °C an hour to 100 °C below the target; then 60 °C an hour to the firing cone; hold 15–30 minutes. Cool naturally; open below 150 °C.
Stoneware glaze, about 1,240–1,300 °C. 150 °C an hour to 1,000 °C (bisqued ware); begin reduction here if you want it (Stoneware and Porcelain); then 60 °C an hour to the firing cone; hold 15–30 minutes. Cool fast to about 1,000 °C to keep glazes bright, then slowly through 600–500 °C and 250–200 °C, where quartz and its high-temperature form (cristobalite) shrink suddenly and can crack the ware.
How to tell it worked
- Cone packs read the same top and bottom, within one number, and the guard cone stands.
- Two firings to the same schedule give the same draw rings and the same ring diameters.
- The thermocouple plot follows the schedule within 25 °C an hour.
- The optical pyrometer agrees with the thermocouple within 15 °C inside a closed kiln.
Note Troubleshooting.
- Cones bend early but glazes are underfired → cones too near the spy hole or in flame; move them where the ware is.
- Firing cone down at the front, ware underfired at the back → uneven kiln. Hold longer at the top; change the setting to let flame through (The Kiln).
- Cones bloat or blister → reduction or coarse grinding; grind finer; calibrate in the atmosphere you fire in.
- Thermocouple reading drifts lower year by year → the wires are being poisoned or oxidised; recalibrate or replace.
Dangers
Danger Your eyes. Staring into kilns and furnaces for years, unprotected, causes cataracts ("glassblower's cataract") from the invisible heat rays. Never look into a kiln above red heat without a dark glass; above 1,200 °C use welding glass or a doubled dark glass. Never look at an electric arc or molten steel without proper welding glass (Welding).
Warning Spy holes blow back. In a smoky, reducing firing, pulling a spy hole plug lets out a jet of flame. Stand to one side and pull plugs with a hooked rod. The gas is carbon monoxide: keep the kiln room ventilated (Chimneys, Stoves and Heating).
- Draw rings come out at 1,000–1,300 °C. Use the long rod, wear leather gloves, and never drop them near your feet. Water quenching spits.
What this unlocks
Repeatable Stoneware and Porcelain, glazes and enamels (Enamel on Metal); production potteries (Slip Casting, Jiggering and Ceramic Factories); controlled heat treatment of steel (Alloy and Stainless Steels); the cone-operated kiln switch and thermocouple controllers of Thermostats and Automatic Control and Electric Kilns and Furnaces; and the measurement of furnace heat everywhere from Glass tanks to Steel in Quantity.
How it was first done
Potters judged heat by colour and draw trials for thousands of years. Josiah Wedgwood made the first measuring pyrometer in 1782, from clay cylinders that shrank in the fire, and was elected to the Royal Society for it. Hermann Seger, a ceramic chemist working for the Royal Porcelain Manufactory in Berlin, published his standardised cones in 1886. In the United States Edward Orton Jr. began making cones at Ohio State University in 1896, and the firm he founded still does. Henri Le Chatelier introduced the platinum thermocouple in 1886 and an optical pyrometer in 1892; the disappearing-filament pyrometer was developed around 1900, by Morse in the United States and by Holborn and Kurlbaum in Germany. Shrinkage rings for the pottery industry followed in the early 20th century.
Source: content/entries/earth/pyrometric-cones.md